Journal of Materials Research and Technology 37 (2025) 64–78 Contents lists available at ScienceDirect Journal of Materials Research and Technology journal homepage: www.elsevier.com/locate/jmrt Influence of SiO2 and Al2O3 content on the phase transformation of vanadium-titanium magnetite pellets in the sodium salt roasting process Wei Liu a , Deqing Zhu a,b,* , Jian Pan a,b , Xiaoman Yang a a b School of Minerals Processing and Bioengineering, Central South University, Changsha, 410083, China Low-carbon and Hydrogen Metallurgy Research Center, Central South University, Changsha, 410083, China A R T I C L E I N F O A B S T R A C T Handling Editor: Prof. M Meyers The influence of SiO2 and Al2O3 concentrations on phase evolution and vanadium recovery within vana­ dium–titanium magnetite pellets during the sodium salt roasting process were investigated. The findings revealed that an increase in SiO2 and Al2O3 levels within the vanadium–titanium magnetite significantly promotes the formation of specific silicates, namely Na1.75Al1.75Si0.25O4 and Na3K(Si0.56Al0.44)O16, as well as aluminates, specifically Na1.22Al11O17.11. The formation of these silicates and aluminates consumes a substantial amount of sodium ions, thereby impeding their diffusion into the interior of vanadium-titanium magnetite particles and suppressing the generation of NaVO3 and Na0.79Fe0.8Ti1.2O4. Additionally, during the sodium salt roasting process, sodium ions migrate from regions of high concentration to those of low concentration via liquid-phase flow and solid-phase diffusion. Elevated SiO2 content and increased roasting temperature both promote slag formation within the pellets. The slag phase fills the interstitial spaces between particles or coats the particle surfaces, promoting the solid solution of vanadium elements into the slag, which is detrimental to the improvement of vanadium leaching rate. Strategic control of SiO2 and Al2O3 levels in vanadium–titanium magnetite can significantly enhance vanadium recovery efficiency. For instance, pellets containing 1.7 % SiO2 and 4.25 % Al2O3, amended with 6 % sodium carbonate and roasted at 1200 ◦ C for 40 min, achieved a vanadium recovery rate of 91.31 %. Keywords: Vanadium-titanium magnetite Vanadium recovery Phase transformation Element migration behavior 1. Introduction Vanadium, often dubbed the "industrial vitamin," is renowned for its ability to significantly bolster the strength of steel alloys [1,2]. In recent years, vanadium batteries have emerged as a promising trend in energy storage technology, driven by their safety and exceptional longevity in cycle life. This development underscores the growing demand for vanadium-containing raw materials [3]. Vanadium–titanium magnetite, which holds 84 % of the world’s vanadium resources, stands out as a crucial feedstock for vanadium extraction [4,5]. Current methodologies for vanadium recovery from vanadiumtitanium magnetite include the blast furnace process, calcification roasting followed by acid leaching, and sodium roasting followed by water leaching [4–6]. In the blast furnace process, vanadium is reduced to its metallic form and dissolved in molten iron. Subsequent treatment in a converter yields vanadium slag, which serves as a source for the production of V2O5. However, due to the protracted process, the blast furnace method typically results in a relatively low overall vanadium recovery rate of around 60 % [4]. Compared to the calcification roasting process, the sodium roasting process circumvents the acid leaching step, achieving selective extraction of vanadium salts through water leaching. This approach also streamlines the purification and enrichment stages of the leaching filtrate. Consequently, the sodium roasting process has gained widespread adoption for vanadium recovery from vana­ dium–titanium magnetite, with industrial vanadium recovery rates exceeding 80 %. Largo Resources Ltd. in Brazil utilizes the sodium roasting process to process vanadium–titanium magnetite, achieving an annual V2O5 processing capacity of approximately 12,000 tons [7]. Bushveld Vametco Ltd. in South Africa employs a rotary kiln roasting method for vanadium–titanium magnetite, with a roasting temperature of approximately 1000 ◦ C and a duration of 3–4 h, achieving vanadium leaching rates of about 80 % [5]. Sodium salt roasting process is a method of oxidative roasting that converts trivalent vanadium in vanadium-titanium magnetite into water-soluble sodium metavanadate [8,9]. In the sodium salt roasting of vanadium-bearing slags and stone coal, the viscosity of the roasting melt * Corresponding author. School of Minerals Processing and Bioengineering, Central South University, Changsha, 410083, China. E-mail addresses: liuweicsu.edu.cn@csu.edu.cn (W. Liu), dqzhu@csu.edu.cn (D. Zhu), pjcsu@csu.edu.cn (J. Pan), 235611067@csu.edu.cn (X. Yang). https://doi.org/10.1016/j.jmrt.2025.05.198 Received 21 March 2025; Received in revised form 15 May 2025; Accepted 22 May 2025 Available online 29 May 2025 2238-7854/© 2025 The Authors. Published by Elsevier B.V. This is an open access article under the CC BY-NC license (http://creativecommons.org/licenses/bync/4.0/). W. Liu et al. Journal of Materials Research and Technology 37 (2025) 64–78 72.68 %. Bian [18] discovered that incorporating K2SO4 hastens the transformation of the mineral structure within vanadium–titanium magnetite. This action promotes the formation of soluble KVO3 while inhibiting the creation of insoluble Ca(VO3)2 during the roasting phase. Additionally, it aids in dissolving sphene and releasing vanadium during leaching, thereby markedly improving vanadium leaching efficiency. Trinh et al. [19] explored the synergistic effects of sodium carbonate with other sodium salts such as Na2SO4 and NaCl in fused salt roasting and found that different combinations of sodium fertilizers could significantly improve vanadium leaching efficiency, reaching up to 71.37 %. Obviously, current research predominantly centers on boosting vanadium recovery from vanadium–titanium magnetite by modifying additives or leaching techniques, with limited exploration of how SiO2 (Al2O3) content affects phase evolution during sodium salt roasting and the migration of sodium salts. Therefore, this manuscript employs a vanadium–titanium magnetite from South Africa to investigate the in­ fluence of SiO2 (Al2O3) content on the sodium salt roasting process of vanadium–titanium magnetite, as well as the migration of sodium salts. Table 1 Chemical composition analysis of vanadium-titanium magnetite (%). TFe FeO CaO MgO SiO2 Al2O3 Na2O 54.48 21.33 0.13 1.46 1.7 4.25 0.071 TiO2 13.35 V2O5 1.62 PbO 0.013 Zn 0.034 S 0.026 P 0.016 LOI − 1.37 K2O 0.019 would be also increased by high SiO2 content, inhibiting the diffusion and release of vanadium oxides [10–13]. High Al2O3 content not only consumes sodium salts but also promotes Al–V solid solution formation. When the SiO2/Al2O3 ratio exceeds 3, a silicate network forms, signifi­ cantly reducing leaching efficiency [14,15]. Unlike vanadium-bearing slags and stone coal, vanadium–titanium magnetite has a simpler mineralogical composition and larger vanadium reserves. Thus, re­ searchers have extensively explored methods to enhance water-soluble sodium vanadate formation to improve the vanadium resource recov­ ery efficiency. Yan [16] used Na2CO3 roasting and mild H2SO4 leaching process to treat vanadium–titanium magnetite with 4.86 % SiO2 and 1.46 % Al2O3. it was observed that Vanadium (V) and impurities like Al and Si were converted into soluble sodium compounds, and some va­ nadium was retained in the sphene phase. Zhang [17] conducted sodium salt roasting of Panxi vanadium–titanium magnetite under a reducing atmosphere at 1200 ◦ C. It was found that most vanadium oxides were converted to sodium vanadate, achieving a vanadium recovery rate of 2. Materials and method 2.1. Materials It can be seen from Table 1 that the content of iron, vanadium, and titanium in the vanadium titanium magnetite are 54.48 %, 1.62 %, and 13.35 %, respectively, indicating a type of vanadium titanium magnetite Fig. 1. Particle morphology (a) and XRD analysis result (b) of vanadium-titanium magnetite. Fig. 2. Element distribution map in vanadium-titanium magnetite. 65 W. Liu et al. Journal of Materials Research and Technology 37 (2025) 64–78 Table 2 The ore blending conditions and roasting temperatures for different groups. NO. S1 S2 S3 S4 S5 S6 S7 S8 S9 S10 S11 S12 S13 S14 S15 The proportion of each raw material in the mixture VTM/% Na2CO3/% 94.34 94.34 94.34 94.34 94.34 94.34 93.34 91.34 89.34 86.34 84.34 93.34 91.34 88.34 86.34 5.66 5.66 5.66 5.66 5.66 5.66 5.66 5.66 5.66 5.66 5.66 5.66 5.66 5.66 5.66 Roasting temperature/◦ C Quartz sand/% Al2O3/% 1.0 3.0 5.0 8.0 10.0 chemical composition of the mixture 800 900 1000 1100 1200 1300 1200 1200 1200 1200 1200 1200 1200 1200 1200 1.0 3.0 6.0 8.0 SiO2/% Al2O3/% 1.6 1.6 1.6 1.6 1.6 1.6 2.58 4.55 6.52 9.47 11.44 4.13 4. 13 4. 13 4. 13 4. 13 4. 13 4.55 5.13 5.97 6.50 Note: VTM is vanadium-titanium magnetite. characterized by high titanium content and low iron content. The con­ tent of Al2O3 and SiO2 within the vanadium titanium magnetite are 4.25 % and 1.7 %, respectively, which are significantly higher than the 0.13 % of CaO. Additionally, as illustrated in Figs. 1 and 2, the primary ironbearing phases in the vanadium titanium magnetite are magnetite and ilmenite, with phlogopite predominantly constituting the gangue min­ erals. The vanadium element is primarily distributed within the ilmenite. 2.2. Methods 2.2.1. Roasting test Initially, 3 kg of dried vanadium–titanium magnetite was weighed and mixed with sodium carbonate, quartz sand (SiO2 content >99.9 %), and Al2O3 in the ratios specified in Table 2. The mixture was homoge­ nized, and water was added as a binder to attain a moisture content of 8.5 %. The mixture was subsequently pelletized using a disc pelletizer. Following the pelletizing protocol for iron ore, the green pellets were screened through 12 mm and 16 mm sieves, with those in the 12–16 mm size range being retained as the final green balls. Following this, the green balls were dried at 105 ◦ C for 3 h. The dried green balls were then roasted in a tube furnace for 40 min. The roasting atmosphere was an air atmosphere, with roasting temperatures ranging from 800 ◦ C to 1300 ◦ C. After roasting, the pellets will be subjected to fine grinding until the proportion of particles with a size less than 0.074 mm exceeds 80 % of the total weight. Particle size analysis was conducted using a standard sieve with a pore size of 0.074 mm. The crushed powder was subse­ quently leached in distilled water at 50 ◦ C for 3 h. The liquid-to-solid ratio was 5:1, and the stirring speed was 200 rpm. After leaching, the slurry is filtered. The filtrate is subjected to chemical analysis, while the filter residue is dried at 105 ◦ C for 10 h in an air-blast-drying oven. Based on the results obtained from the chemical analysis, the vanadium leaching efficiency is calculated using the following equation [20]: R = (V⋅C) × 100%/(m0 ⋅α0 ) Fig. 3. Stacking dium carbonate. diagram of vanadium-titanium magnetite with so­ 2.2.3. Sodium salt migration assay To investigate whether sodium salt migrates within the mineral phase, 10 g of vanadium-titanium magnetite was formed into cylindrical pellets measuring 300 mm in diameter and 2 mm in thickness, using a mold. An additional sodium carbonate, SiO2 or Al2O3 were prepared into cylindrical pellet with a diameter of 100 mm and a thickness of 2 mm. The weights of Na2CO3, SiO2 and Al2O3 are all 5g. The sodium car­ bonate, SiO2 or Al2O3 and vanadium-titanium magnetite were stacked on a 500 mm diameter corundum tile as depicted in Fig. 3. Following drying at 105 ◦ C for 3 h, the setup was roasted in a tube furnace at 1200 ◦ C for 40 min. The roasted melt was prepared as a thin section for phase observation. 2.2.4. Microstructure and composition The effects of different iron grades on the microstructure and composition of reduced pellets were studied studied by using Scanning electron microscopy (SEM, Nova NanoSEM 450, America) and energy spectrometer (EDS, AZtec X-MaxN80, England). Additionally, X-ray diffraction (XRD, SIMENS D500, Germany) was used to investigate the changes in crystal composition during the reduction process of the pellets. (1) Where R is the recovery rate of vanadium in the leaching solution, %; V is the volume of the leaching solution, L; C is the concentration of V in the leaching solution, g/L; m0 is the mass of roasted sample used in each experiment, g; α0 is the content of V in the roasted sample, %. 3. Results and discussion 2.2.2. Thermodynamic calculation The potential chemical reactions and phase transition processes within vanadium titanium-magnetite pellets were computed using the Reaction module and Phase Diagram module within FactSage 8.0, respectively. The calculation was conducted under standard atmo­ spheric pressure. 3.1. Thermodynamic calculation During sodium salt roasting of stone coal and vanadium-containing slag, SiO2 and Al2O3 in the minerals consume sodium salts, promoting 66 W. Liu et al. Journal of Materials Research and Technology 37 (2025) 64–78 Fig. 4. Thermodynamic calculation result (a-the binary phase diagram of SiO2–Al2O3 with the mass of 6 % Na2O; b-The quaternary phase diagram of Na2O–SiO2–Al2O3–V2O5 at 1200 ◦ C; The quaternary phase diagram of Na2O–SiO2–Al2O3–V2O5 at 1300 ◦ C). low-melting-point compound formation. This alters the mineral struc­ ture and impacts vanadium leaching efficiency. Vanadium–titanium magnetite’s impurities are mainly silicates like mica, garnet, and py­ roxene [4,7,16–19]. To theoretically explore how varying SiO2 and Al2O3 contents affect the slag phase composition in sodium salt–laden vanadium–titanium magnetite pellets, the phase composition of the SiO2–Al2O3–Na2O ternary system and the SiO2–Al2O3–Na2O -V2O5 quaternary system at different temperatures were calculated using FactSage software. As illustrated in Fig. 4a, when the Na2O content is 6.0 %, and the SiO2 content in SiO2–Al2O3–Na2O system is no higher Fig. 5. Effect of SiO2 (a) and Al2O3 (b) contents on the phasor of slag in vanadium titanium magnetite pellets. 67 W. Liu et al. Journal of Materials Research and Technology 37 (2025) 64–78 Fig. 6. Effect of roasting temperature (a) on recovery of vanadium in leaching filtrate and the phase transformations (b). than 17.2 %, silicon, aluminum, and sodium elements predominantly exist in the forms of NaAl9O14 and nepheline. At temperatures exceeding 1269.6 ◦ C, the formation of liquid slag begins. Concurrently, at 1200 ◦ C, as depicted in Fig. 4b, the addition of V2O5 to the SiO2–Al2O3–Na2O ternary system results in a coexistence region where sodium vanadate (Na3VO4) and liquid slag are present within the SiO2–Al2O3–Na2O ternary system. This observation implies that within the specified re­ gion, vanadium predominantly exists in the form of Na3VO4, which is not incorporated into the slag phase. This is evidently conducive to the efficient leaching of vanadium in subsequent processes. However, this region disappears when the temperature rises to 1300 ◦ C and is replaced by the slag phase. This also implies that even if SiO2 and Al2O3 are present at specific content levels, too high a temperature will still lead to the formation of the slag phase, which will hinder the stable existence of vanadate or metavanadate. In addition, FactSage calculations based on the composition detailed in Table 2 reveal that an increase in aluminum content and a decrease in silicon content is beneficial in reducing the formation of the slag phase in vanadium-titanium magnetite at elevated temperatures, as illustrated in Fig. 5. Additionally, as illustrated in Fig. 5, the slag content within the pellets rapidly increases to over 30 % when the temperature rises from 1250 ◦ C to 1300 ◦ C. At 1250 ◦ C, when the SiO2 content is below 2.58 % and the Al2O3 content ranges between 4.13 % and 6.5 %, the slag phase in vanadium-titanium magnetite pellets is maintained below 10 %. The presence of a low slag content is advantageous for the stable existence of vanadate. LI et al. argued that the formation of high-temperature liquids negatively affects the oxidation and leaching of vanadium [21]. How­ ever, Yi et al. [22] thought that the liquid formation may also have positive influences: it can accelerate the diffusion of sodium salt and concentrate vanadium to local areas. 3.2. Effect of roasting temperature on recovery of vanadium The chemical reactions that take place during the sodium oxidation roasting of vanadium-titanium magnetite encompass the oxidation of magnetite, the formation of metavanadate, the oxidation of ilmenite, and the formation of silicate, among others [20,22,23]. The specific chemical equations are detailed in Eq. (2) to Eq. (7). The optimal roasting temperature varies for different types of vanadium-titanium magnetite due to their distinct mineral compositions. As depicted in Fig. 6, the vanadium recovery rate in the leaching solution exhibits an initial increase followed by a decrease as the roasting temperature is raised from 800 ◦ C to 1300 ◦ C. The recovery of vanadium in the leaching solution can exceed 90 % when the roasting temperature is maintained between 1100 ◦ C and 1200 ◦ C. However, in the sodium salt roasting and water leaching treatment process of vanadium-titanium magnetite, the recommended roasting temperature is 800 ◦ C–1000 ◦ C, with the roast­ ing time typically ranging from 1 to 4 h [20,24]. Furthermore, it is believed that excessive roasting temperatures leading to "sintering" can exacerbate the improvement of the vanadium leaching rate. The use of sodium salts promotes the formation of low-melting silicates, which can encase iron ore particles, thereby reducing the vanadium leaching rate [20,23]. The discrepancy between the two processes is attributed to the varying chemical compositions of vanadium-titanium magnetite. As illustrated in Table 3 and Fig. 5, the vanadium–titanium magnetite investigated in this manuscript has a lower SiO2 content and a higher Al2O3 content. These characteristics appear to reduce the formation of liquid phase during roasting at temperatures ranging from 1100 ◦ C to 1200 ◦ C [25]. Moreover, this also provides the possibility for increasing the roasting temperature. 2Fe3 O4 + 0.5O2 = 3Fe2 O3 (2) Table 3 Results of sodium salt roasting of vanadium-titanium-magnetite in different literatures. Reference Chemical composition of raw materials/% TFe SiO2 Al2O3 TiO2 V2O5 CaO MgO Ref.4[16] Ref.2[20] 48.19 51.65 4.68 6.06 1.46 2.13 20.42 13.92 0.83 1.55 2.47 2.80 0.37 0.52 Ref.5[22] Ref.1[30] Ref.3[31] TM* 57.92 44.2 46.79 54.48 3.69 9.85 6.54 1.7 2.83 3.14 2.28 4.25 6.25 19.72 18.9 13.35 0.71 1.10 1.71 1.62 0.76 4.71 2.91 0.13 2.55 0.78 0.9 1.46 Dosage of additive Roasting temperature/◦ C Roasting time/h Leaching rate/ % Leaching method 5 % Na2CO3 4 % Na2CO3+ 3 % CaCO3 8 % Na2SO4 4 % K2SO4 7.5 % Na2CO3 6 % Na2CO3 900 950 3.0 4.0 91.0 75.19 Sulfuric acid Sulfuric acid 1200 900 850 1200 0.33 1.0 4.0 0.66 85.6 % 71.37 85.0 91.31 Water Sulfuric acid Water Water Note: TM* represents experimental data in this draft. 68 W. Liu et al. Journal of Materials Research and Technology 37 (2025) 64–78 Fig. 7. SEM-EDS analysis results of the leaching residue from vanadium titanomagnetite roasted at 900 ◦ C. Na2 CO3 + V2 O3 + O2 = CO2 + 2NaVO3 (3) 2FeTiO3 + 0.5O2 = 2TiO2 + Fe2 O3 (4) Na2 CO3 + SiO2 = Na2 SiO3 + CO2 (5) Na2 CO3 + Al2 O3 = 2NaAlO2 + CO2 (6) Na2 CO3 + Al2 O3 + 2SiO2 = 2NaAlSiO4 + CO2 (7) aqueous solution, further fine grinding is evidently required. With further increases in roasting temperature, the dispersion of silicate is enhanced, and some silicon and aluminum elements begin to be more thoroughly incorporated into ilmenite, as shown in the microregion at spot 5 of Fig. 9. Vanadium elements are "dissolved" into sodium silicate. this suggests that excessively high temperatures, by intensifying the dispersion of silicate, lead to the dissolution of vanadium into it, thereby increasing the residual vanadium content in the filter slag [28,29]. The phase transformations of vanadium-titanium magnetite during roasting are depicted in Fig. 6b. As the roasting temperature rises from 800 ◦ C to 1300 ◦ C, ilmenite undergoes gradual oxidation, transitioning through the phase changes of FeTiO3 → Fe1.5Ti0.5O3 → Fe2TiO5. Furthermore, the temperature increase facilitates the "migration" of sodium ions into the ilmenite lattice, leading to the formation of Na0.79(Fe0.8Ti1.2O4), which appears to be beneficial for the conversion of vanadate within ilmenite. Intriguingly, the elevation in roasting tem­ perature also appears to enhance the formation of Na3K (Si0.56Al0.44)8O16. The microstructural analysis of the filter slag from vanadiumtitanium magnetite treated at various roasting temperatures is pre­ sented in Figs. 7–9. Observations from these figures reveal that at a roasting temperature of 900 ◦ C, a portion of the ilmenite within the iron ore particles still retains a significant amount of vanadium, suggesting that the sodium oxidation of vanadium in some ilmenite is incomplete [26,27]. As the roasting temperature is elevated to 1200 ◦ C, there is a noticeable reduction in the residual vanadium content in the filter slag, with vanadium distribution primarily coinciding with sodium and being dispersed among silicate or iron ore particles. Silicate is found inter­ spersed among iron ore particles in irregular lumps or strips, without forming a distinct enveloping structure around hematite particles. This indicates that the residual vanadium in the filter slag is likely due to particles that have not been finely ground to the desired grain size. The microregion at spot 3 in Fig. 8 still contains a small amount of NaVO3, which is distributed between the particles. To facilitate its dissolution in 3.3. Effect of SiO2 and Al2O3 content on recovery of vanadium The recovery of vanadium in the leaching solution is negatively correlated with the silicon content in vanadium-titanium magnetite. As depicted in Fig. 10, the vanadium recovery rate in the leaching solution plummets from 91.79 % to 2.1 % as the silicon content rises from 1.6 % to 11.44 %. Furthermore, when the silicon content in the pellets reaches 4.55 %, the vanadium leaching rate was significantly reduced to 57.4 %. this phenomenon may be attributed to the fact that the increase in SiO2 content has changed the microscopic composition of the mineral. As depicted in Fig. 10b, the number of diffraction peaks for the Na3K (Si0.56Al0.44)O16 significantly increases in the pellets after roasting. This change leads to substantial consumption of sodium salts, thereby hin­ dering the formation of water-soluble vanadate [20,27]. Meanwhile, Fig. 11a reveals that silicates not only fill the interstitial spaces between iron ore particles but also encapsulate some fine hematite particles. The distribution of vanadium elements highly coincides with that of silicon and aluminum elements, indicating that vanadium has been incorpo­ rated into the silicates, which directly results in a decreased vanadium leaching rate. Moreover, due to the enrichment of sodium salts in sili­ cates, the interaction between vanadium elements and sodium ions within the particles is inhibited, causing a higher coincidence of vana­ dium elements with titanium elements than with sodium elements, as shown in Fig. 11b. In Fig. 11b, microregions of spot 4 and spot 5 contain almost no sodium elements but have a small amount of vanadium ele­ ments, which further confirms that sodium elements have not diffused 69 W. Liu et al. Journal of Materials Research and Technology 37 (2025) 64–78 Fig. 8. SEM-EDS analysis results of the leaching residue from vanadium titanomagnetite roasted at 1200 ◦ C. into the interior of the particles, while vanadium elements remain within the particles. Zhang [23] also reached a similar conclusion, suggesting that this portion of vanadium still exists in the form of V(III). The effect of Al2O3 content on the sodium salt roasting of vanadiumtitanium magnetite is analogous to that of SiO2. Fig. 12 demonstrates that as the Al2O3 content increases from 2.58 % to 6.50 %, the vanadium recovery rate drops from 91.31 % to 42.74 %. Furthermore, an increase in Al2O3 content not only leads to the formation of sodium aluminosil­ icate salts (Na1.75Al1.75Si0.25O4) but also fosters the creation of sodium aluminate (Na1.22Al11O17.11), which "consumes" free Na2O, thereby reducing the content of the Na0.79(Fe0.8Ti1.2O4) phase. This observation is further supported by the elemental distribution of Na, Ti, and V as 70 W. Liu et al. Journal of Materials Research and Technology 37 (2025) 64–78 Fig. 9. SEM-EDS analysis results of the leaching residue from vanadium titanomagnetite roasted at 1300 ◦ C. shown in Fig. 13. Microregions of spot 3 in Fig. 13 contain a small amount of vanadium elements, which hinders the increase of the V leaching rate. The primary difference lies in the fact that an elevated Al2O3 content seems to augment the solid solution of Al3+ in ilmenite, thereby raising the Al content within ilmenite. This implies that the interaction between vanadium in ilmenite and Na+ is weakened, which is unfavorable for the migration of vanadium within ilmenite. In summary, as the content of SiO2 and Al2O3 increases, sodium salts 71 W. Liu et al. Journal of Materials Research and Technology 37 (2025) 64–78 Fig. 10. Influence of SiO2 content on vanadium recovery (a) and mineral phase composition(b) at 1200 ◦ C. Fig. 11. SEM-EDS analysis results of the leaching residue from vanadium titanomagnetite with 4.55 % SiO2. 72 W. Liu et al. Journal of Materials Research and Technology 37 (2025) 64–78 Fig. 12. Influence of Al2O3 content on vanadium recovery (a) and mineral phase composition(b) at 1200 ◦ C. Fig. 13. SEM-EDS analysis results of the leaching residue from vanadium titanomagnetite with 5.97 % Al2O3. 73 W. Liu et al. Journal of Materials Research and Technology 37 (2025) 64–78 Table 4 EDS analysis results of selected microregions in Fig. 14/(wt. %). Spectrum No. O Na Mg Al Si Ca Ti V Fe Mineral phase 1 2 3 4 5 6 7 8 9 10 11 21.77 6.37 30.97 11.14 12.99 7.59 11.62 11.28 12.97 11.07 13.79 19.38 21.52 37.88 12.32 13.47 15.75 25.5 28.28 2.2 13.94 11.42 1.19 1.88 0.48 0.21 1.5 0.51 0.45 0.33 0.63 0.46 0 4.36 2.46 0.6 5.16 3.8 1.54 7.12 2.64 1.04 3.72 4.75 2.69 0.27 0 0.85 0.29 0 0.37 0 0 1.66 1.55 1.07 1.18 0.51 2.17 0.35 0.19 3 0.54 0 0.17 0.39 23.14 5.24 2.04 23.47 4.64 2.64 2.2 11.43 6.11 5.92 21.87 5.8 10.16 17.94 9.56 3.35 4.35 31.17 16.47 0.43 2.62 8.1 20.6 50.93 9.58 35.12 59.6 67.43 18.56 29.03 76.62 60.45 38.13 Ilmenite Hematite NaVO3 Ilmenite Hematite Hematite NaVO3 Ilmenite Hematite Hematite Ilmenite Table 5 EDS analysis results of selected microregions in Fig. 15/(wt. %). Spectrum No. O Na Mg Al Si Ca Ti V Fe Mineral phase 1 2 3 4 5 6 29.02 22.87 10.64 18.98 13.89 17.12 0 14.6 1.06 18.12 0 0 0 0 0.78 0 0.36 0.97 0 0.78 1.16 3.93 1.13 1.85 70.37 44.54 0 11.21 0 0 0 0 0 0.3 0 0 0 0 5.98 23.2 11.21 9.34 0 0.58 0.29 2.7 1.54 1.45 0.61 16.62 80.09 21.55 71.88 69.27 Quartz Olivine Hematite Ilmenite Hematite Hematite Table 6 EDS analysis results of selected microregions in Fig. 16/(wt. %). Spectrum No. O Na Mg Al Si Ca Ti V Fe Mineral phase 1 2 3 4 5 6 21.17 11.64 8.62 20.24 8.85 15.45 15.38 0 0 14.64 0 9.31 0 0.93 0.87 0 0 4.36 18.95 0.95 1.21 5.61 0.91 5.2 28.65 0 0 4.47 0 5.62 0 0 0 0 0 0.41 1.65 5.95 5.01 31.57 2.18 12.55 0 0.47 0.39 0 0 1.24 14.2 80.07 83.9 23.48 88.06 45.88 silicate Hematite Hematite Ilmenite Hematite Ilmenite Fig. 14. Migration results of sodium in vanadium-titanium magnetite at 1200 ◦ C. are consumed to form sodium silicate or sodium aluminate, thereby inhibiting the reaction between V elements and Na ions within the particles. Meanwhile, the increased content of silicates between parti­ cles also increases the likelihood of some vanadium elements being solid-solved into the inter-particle silicates, which is clearly detrimental to the formation and stable presence of vanadate [23,32]. 3.4. Migration behavior of sodium Upon comparing Figs. 14–16 and Tables 4–6, it becomes evident that sodium in vanadium-titanium-magnetite exists in three primary forms: sodium metavanadate, sodium aluminosilicate, and Fe0.8Na0.79Ti1.2O4. Sodium salts migrate from high-concentration central areas to the 74 W. Liu et al. Journal of Materials Research and Technology 37 (2025) 64–78 Fig. 15. Migration results of sodium in vanadium-titanium-magnetite at 1200 ◦ C after the addition of SiO2. periphery during roasting, as illustrated in Fig. 14 and Table 4 The distribution of sodium salts reveals that their migration behavior in­ volves the flow of sodium ions through the low-melting-point slag phase between iron ore particles, as well as the solid-phase diffusion of sodium elements within ilmenite. Furthermore, sodium ions combine with oxidized V2O5 to form metavanadate during migration. Local statistical results indicate that sodium ions are uniformly distributed across the vanadium-titanium-magnetite cluster region, suggesting that the mobility of sodium elements is driven by regional concentration dif­ ferences, as shown in Figs. 14a and c and Table 4. The increase in Al2O3 and SiO2 contents in vanadium-titanium magnetite leads to greater enrichment of sodium ions in aluminosili­ cate, as shown in Fig. 16. By comparing the element distribution in the external microregions in Figs. 15 and 16, it can be found that Al2O3 is more favorable for the outward diffusion of Na element. This is due to the fact that the bond energy of the Al - O bond is relatively lower compared to that of the Si - O bond. At high temperatures, sodium aluminate exhibits relatively high reactivity, allowing it to interact with the surrounding particles more rapidly and migrate to other locations [33,34]. By comparing the distribution of elements in regions b and c in Fig. 15, it is evident that the silicon and sodium content in region c is significantly reduced. This phenomenon arises from the reaction be­ tween Na2O and SiO2, which forms low-melting-point silicates. At higher roasting temperatures, these silicates melt into a liquid phase and fill the interstitial spaces between particles, indicating that the migra­ tion of sodium within the silicates also relies on liquid-phase flow [22, 35,36]. In contrast, sodium aluminate is primarily transferred through the solid phase, resulting in a more uniform distribution of sodium ions as seen in Fig. 16. This phenomenon bears a resemblance to the mech­ anism observed in iron ore pellets. During the high-temperature roasting process, ions acquire enough energy to surmount the bond forces that typically constrain them, thereby enhancing their diffusion capacity [37, 38]. Building upon the aforementioned analysis and the migration behavior of sodium salts, it can be further deduced that the migration of sodium salts within vanadium - titanium - magnetite pellets is markedly affected by the content of SiO2 and Al2O3. Consistent with the analysis in Section 3.3, when the gangue mineral content in vanadium–titanium magnetite is low, sodium ions are more likely to diffuse into the particle interiors, thereby facilitating the formation of additional water-soluble 75 W. Liu et al. Journal of Materials Research and Technology 37 (2025) 64–78 Fig. 16. Migration results of sodium elements in vanadium-titanium magnetite after the addition of Al2O3 at 1200 ◦ C. Fig. 17. The correlation between sodium and vanadium elements before (a) and after (b) the addition of SiO2 and Al2O3. 76 W. Liu et al. Journal of Materials Research and Technology 37 (2025) 64–78 vanadate. This also indicates that under these conditions, the migration of sodium ions may be primarily driven by solid-phase diffusion. How­ ever, as the gangue mineral content increases, sodium becomes enriched in silicate, inhibiting the diffusion of sodium salts into the interior of ilmenite particles. This reduces the formation of the Fe0.8Na0.79Ti1.2O4 phase and promotes the dissolution of vanadium into silicate, thereby diminishing the presence of water-soluble vanadate. Therefore, without considering the influence of calcium and magnesium elements, reducing the SiO2 and Al2O3 content in vanadium-titanium magnetite emerges as an effective strategy to enhance the vanadate brine leaching process. An increase in the content of SiO2and Al2O3 will impede the reaction between vanadium(V) and sodium (Na). through the statistical and analytical assessment of the EDS results from Table 4, it was observed that a high correlation between sodium (Na) and vanadium (V) ele­ ments, indicating that sodium ions primarily interacted with vanadium. However, upon the addition of SiO2 and Al2O3, the association of sodium ions with [Si + Al] elements increased, thereby reducing the correlation between sodium and vanadium, as shown in Fig. 17. This suggests that the incorporation of SiO2 and Al2O3altered the chemical environment of sodium ions, causing them to preferentially bond with silicate, thus affecting the interaction between sodium and vanadium. South University, National Key R&D Program of China (2023YFC3903900,2023YFC3903904), Innovation-driven Project of Guangxi Zhuang Autonomous Region (2024AA08010-2), and Funda­ mental Research Funds for the Central Universities of Central South University, China (No. 2024ZZTS0427). References [1] Hu P, Hu P, Vu TD, Li M, Wang S, Ke Y, Zeng X, Mai L, Long Y. Vanadium oxide: phase diagrams, structures, synthesis, and applications. Chem Rev 2023;123(8): 435. https://doi.org/10.1021/acs.chemrev.2c00546. [2] Yang MQ, Yang JY. Vanadium extraction from steel slag: generation, recycling and management. Environ Pollut 2024;343:123126. https://doi.org/10.1016/j. envpol.2023.123126. [3] An Y, Ma B, Li X, Chen Y, Wang C, Wang B, Gao M, Feng G. A review on the roasting-assisted leaching and recovery of V from vanadium slag. Process Saf. Environ 2023;173:263. https://doi.org/10.1016/j.psep.2023.03.013. [4] Peng H. A literature review on leaching and recovery of vanadium. J Environ Chem Eng 2019;7(5):103313. https://doi.org/10.1016/j.psep.2023.03.013. [5] Moskalyk RR, Alfantazi AM. Processing of vanadium: a review. Miner Eng 2003;16 (9):793. https://doi.org/10.1016/S0892-6875(03)00213-9. [6] Petranikova M, Tkaczyk AH, Bartl A, Amato A, Lapkovskis V, Tunsu C. Vanadium sustainability in the context of innovative recycling and sourcing development. Waste Manage (Tucson, Ariz) 2020;113:521. https://doi.org/10.1016/j. wasman.2020.04.007. [7] Chen Dong-hui. Vanadium industry 2022 annual evaluation. Journal of hebei metallurgy 2023;(12):1. https://doi.org/10.13630/j.cnki.13-1172.2023.1201. [8] Stander PP, Van Vuuren CPJ. The high temperature oxidation of FeV2O4. Thermochim Acta 1990;157(2):34. https://doi.org/10.1016/0040-6031(90) 80036-X. [9] Van Vuuren CPJ, Stander PP. The oxidation of FeV2O4 by oxygen in a sodium carbonate mixture. Miner Eng 2001;14(7):803. https://doi.org/10.1016/S08926875(01)00076-0. [10] Liu S, Wang L, Chen J, Ye L, Du J. Research progress of vanadium extraction processes from vanadium slag: a review. Sep Purif Technol 2024;342:127035. https://doi.org/10.1016/j.seppur.2024.127035. [11] Li C, Jiang T, Wen J, Yu T, Li F. Review of leaching, separation and recovery of vanadium from roasted products of vanadium slag. Hydrometallurgy (Amst) 2024; 226:106313. https://doi.org/10.1016/j.hydromet.2024.106313. [12] Wang M, Huang S, Chen B, Wang X. A review of processing technologies for vanadium extraction from stone coal. Miner Process Extr M 2020;129(3–4):290. https://doi.org/10.1080/25726641.2018.1505207. [13] Zhang YM, Bao SX, Liu T, Chen TJ, Huang J. The technology of extracting vanadium from stone coal in China: history, current status and future prospects. Hydrometallurgy (Amst) 2011;109(1–2):116. https://doi.org/10.1016/j. hydromet.2011.06.002. [14] Mingyu W, Xiang X, Zhang L, Liansheng X. Effect of vanadium occurrence state on the choice of extracting vanadium technology from stone coal. Rare Met 2008;27 (2):112. https://doi.org/10.1016/S1001-0521(08)60097-2. [15] Wang YH, Wang YF, Li YT, Wu C, Han XL, Zhao NN, He ZX. A review on vanadium extraction techniques from major vanadium-containing resources. Rare Met 2024; 43(9):4115. https://doi.org/10.1007/s12598-024-02721-w. [16] Yan Z, Zheng S, Zhang Y, Zhang Y, Zhou Z, Qiao S. Sodium carbonate roasting and mild acid leaching of vanadium titanomagnetite concentrates: vanadium extraction and residue sodium decrease. Process Saf Environ 2024;185:1132. https://doi.org/ 10.1016/j.psep.2024.03.046. [17] Zhang YM, Wang LN, Chen DS, Wang WJ, Liu YH, Zhao HX, Qi T. A method for recovery of iron, titanium, and vanadium from vanadium-bearing titanomagnetite. Int J Min Met Mater 2018;25:131. https://doi.org/10.1007/s12613-018-1556-0. [18] Bian Z, Ning Z, Zhao K, Gao R, Li W, Lv C, Yuan Y, Li H. Recovery of vanadium, titanium, and iron from vanadium titanomagnetite concentrate through ammonium sulfate cascade roasting with potassium pyrosulfate. J Sustain Metall 2022;8(4):1988. https://doi.org/10.1007/s40831-022-00627-4. [19] Trinh HB, Kim S, Lee J, Oh S. Efficient recovery of vanadium and titanium from domestic titanomagnetite concentrate using molten salt roasting and water leaching. Materials (Basel) 2023;16(21):6918. https://doi.org/10.3390/ ma16216918. [20] Bai L, Xiang J, Lu X, Xu Y, Zhu K, Yu J, Lv X. Extraction of vanadium from vanadium–titanium magnetite: enhanced by sodium–calcium synergistic roastingwater leaching process. Metall Mater Trans B 2025;56:552. https://doi.org/ 10.1007/s11663-024-03369-8. [21] Ren-min LI, Liu Tao, Yi-min ZHANG, Huang Jing, Cheng-bao XU. Efficient extraction of vanadium from vanadium− titanium magnetite concentrate by potassium salt roasting additives. Minerals (Basel) 2018;8(1):25. https://doi.org/ 10.3390/min8010025. [22] Yi YH, Hu SUN, You JX, Zhang J, Yuan CAI, Zhang X, Qiu GZ. Vanadium recovery from Na2SO4-added V-Ti magnetite concentrate via grate-kiln process. T Nonferr Metal Soc 2022;32(6):2019. https://doi.org/10.1016/j.jmrt.2021.11.039. [23] Zhang S, Li G, Xiao R, Luo J, Yi L, Rao M. Extraction of vanadium from lowvanadium grade magnetite concentrate pellets with sodium salt. J Mater Res Technol 2021;15:5712. https://doi.org/10.1016/j.jmrt.2021.11.039. [24] Gao F, Du H, Wang S, Chen B, Li J, Zhang Y, Olayiwola AU. A comparative study of extracting vanadium from vanadium titano-magnetite ores: calcium salt roasting vs 4. Conclusions 1. As the content of SiO2 and Al2O3 increases, sodium salts are consumed, and the process of sodium oxidation of vanadium ele­ ments within the particles is hindered. Meanwhile, vanadium ele­ ments are more likely to be solid-solved into silicates. These factors are all detrimental to increasing the vanadium leaching rate. This issue can be mitigated by optimizing the roasting temperature and controlling the SiO2 and Al2O3 content in vanadium-titanium magnetite. 2. An increase in the SiO2 and Al2O3 content in vanadium-titanium magnetite leads to a higher concentration of silicate phases (Na1.75Al1.75Si0.25O4 or Na3K(Si0.56Al0.44O16)) and sodium aluminate (Na1.22Al11O17.11) in the pellets. These phases hinder the migration of sodium ions into particles, resulting in a decrease in the Fe0.8Na0.79Ti1.2O4 phase and a progressive increase in the Fe2TiO5 phase. 3. Sodium ions in vanadium-titanium magnetite migrate toward re­ gions with lower sodium content through the flow of low-melting slag phases or solid-phase diffusion. sodium salts mainly occur in silicate, sodium iron titanate, and sodium vanadate phases in the pellets, and an increase in SiO2 and Al2O3 contents curtail sodium distribution in sodium titanate and sodium vanadate. CRediT author statement For research article with several authors, a short paragraph speci­ fying their individual contributions have been provided. Funding acquisition, Jian Pan, Deqing Zhu; Investigation, Wei Liu, Xiaoman Yang; Methodology, Jian Pan and Deqing Zhu; Supervision, Jian Pan, Deqing Zhu; Writing – original draft, Wei Liu; Writing – review & edit­ ing, Wei Liu and Deqing Zhu. Declaration of interest statement There is no conflict. the paper submitted is the result of the discus­ sion between myself and the relevant authors. Except for the content specifically cited in the paper, the paper does not contain any other published or written works by individuals or groups. Acknowledgements The authors gratefully acknowledge the financial supported by the Fundamental Research Funds for the Central Universities of Central 77 W. Liu et al. Journal of Materials Research and Technology 37 (2025) 64–78 Sources, Part A Recovery, Util Environ Eff 2018;40(17):1998. https://doi.org/ 10.1080/15567036.2018.1486907. [32] Gilligan R, Nikoloski AN. The extraction of vanadium from titanomagnetites and other sources. Miner Eng 2020;146:106106. https://doi.org/10.1016/j. mineng.2019.106106. [33] Shi S, Gao L, Zhang J, He Z. New insights on consolidation behavior of Fe2O3 in the Fe3O4-CaO-MgO-SiO2 system for fluxed pellet production: phase transformations and morphology evolution. Miner Eng 2024;214:108797. https://doi.org/ 10.1016/j.mineng.2024.108797. [34] Li XB, Wang YL, Zhou QS, Qi TG, Liu GH, Peng ZH, Wang HY. Reaction behaviors of iron and hematite in sodium aluminate solution at elevated temperature. Hydrometallurgy (Amst) 2018;175:257. https://doi.org/10.1016/j. hydromet.2017.12.00. [35] Neuville DR. Viscosity, structure and mixing in (Ca, Na) silicate melts. Chem Geol 2006;229(1–3):28. https://doi.org/10.1016/j.chemgeo.2006.01.008. [36] Yu L, Dong YC, Ye GZ, Sichen D. Concentrating of vanadium oxide in vanadium rich phase (s) by addition of SiO2 in converter slag. Ironmak Steelmak 2007;34(2): 131. https://doi.org/10.1179/174328107x155286. [37] Zhu D, Yang C, Pan J, Zhang Q, Shi B, Zhang F. Insight into the consolidation mechanism of oxidized pellets made from the mixture of magnetite and chromite concentrates. Metall Mater Trans B 2016;47:1010. https://doi.org/10.3390/ pr7120931. [38] Li H, Wu S, Hong Z, Zhang W, Zhou H, Kou M. The mechanism of the effect of Al2O3 content on the liquid phase fluidity of iron ore fines. Processes 2019;7(12): 931. https://doi.org/10.3390/pr7120931. sodium salt roasting. Miner Process Extr M 2023;44(5):352. https://doi.org/ 10.1080/08827508.2022.2069105. [25] Guo Y, Liu K, Chen F, Wang S, Yang L, Li D, Zheng Y. Effect of high-pressure grinding rolls pretreatment on the preparation of vanadium-titanium magnetite pellets. J Mater Res Technol 2023;23:2479. https://doi.org/10.1016/j. jmrt.2023.01.125. [26] Pan F, Zhu QS, Du Z, Sun HY. Oxidation kinetics, structural changes and element migration during oxidation process of vanadium-titanium magnetite ore. J Iron Steel Res Int 2016;23(11):1160. https://doi.org/10.1016/S1006-706X(16)301716. [27] Sui Y, Guo Y, Jiang T, Qiu GZ. Separation and recovery of iron and titanium from oxidized vanadium titano-magnetite by gas-based reduction roasting and magnetic separation. J Mater Res Technol 2019;8(3):3036. https://doi.org/10.1016/j. jmrt.2018.05.031. [28] Zeng X, Wang F, Zhang H, Cui L, Yu J, Xu G. Extraction of vanadium from stone coal by roasting in a fluidized bed reactor. Fuel (Guildf) 2015;142:180. https://doi. org/10.1016/j.fuel.2014.10.068. [29] Cheng G, Li L, Xue X, Yang H, Zhang W, Bai R. Effects of extracted-vanadium residue and MgO on the basic sintering characteristics of high-chromium vanadium–titanium magnetite. J Mater Res Technol 2022;17:2657. https://doi. org/10.1016/j.jmrt.2022.01.144. [30] Li R, Liu T, Zhang Y, Huang J, Xu C. Efficient extraction of vanadium from vanadium–Titanium magnetite concentrate by potassium salt roasting additives. Minerals (Basel) 2018;8(1):25. [31] Luo XF, Dong H, Zhang S, Liu YW. Study on the sodium oxidation properties of low-iron vanadium-titanium magnetite with high vanadium and titanium. Energy 78
0
You can add this document to your study collection(s)
Sign in Available only to authorized usersYou can add this document to your saved list
Sign in Available only to authorized users(For complaints, use another form )