Thin-Walled Structures 49 (2011) 1534–1543 Contents lists available at SciVerse ScienceDirect Thin-Walled Structures journal homepage: www.elsevier.com/locate/tws Concrete-filled double skin steel tubular (CFDST) columns subjected to long-term sustained loading Lin-Hai Han n, Yong-Jin Li, Fei-Yu Liao Department of Civil Engineering, Tsinghua University, Beijing 100084, PR China a r t i c l e i n f o a b s t r a c t Article history: Received 10 October 2010 Received in revised form 29 July 2011 Accepted 3 August 2011 Available online 27 August 2011 This paper carried out a series of tests on concrete-filled double skin steel tubes (CFDST) columns under long-term sustained loading condition. The test process included two stages, i.e. long-term service test and ultimate strength test. Numerical models on analysis of the CFDST column under long-term sustained loading were presented. A comparison of results calculated using these models showed generally good agreement with the test results. Additionally, a detailed analysis was performed to analyse the long-term behaviour of CFDST columns. Finally, simplified formula for calculating the ultimate strength of CFDST columns subjected to long-term sustained loading was proposed. & 2011 Elsevier Ltd. All rights reserved. Keywords: Concrete-filled double skin tube (CFDST) Concrete filled steel tube(CFST) Concrete Column Long-term sustained loading Ultimate strength Parametric analysis 1. Introduction Concrete-filled double skin steel tube (CFDST) columns have been recognised to have a series of advantages, such as high strength and bending stiffness, good seismic and fire performance, and favourable construction ability [1]. Fig. 1(a) and (b) shows two typical profiles of the CFDST sections (named as circular CFDST and square CFDST), where hollow ratio (w) of the CFDST sections was defined as follows [2,3]: w¼ Di Do 2to ð1aÞ w¼ Di Bo 2to ð1bÞ where Do and Di are the diameters of outer and inner circular steel tube, respectively; Bo is the width of outer square steel tube; to and ti are the thicknesses of outer and inner steel hollow section, respectively, as shown in Fig.1. CFDST columns have potential to be used as column or pier in structures. The behaviour of CFDST columns under short-term loading has been the subject of investigations, such as Zhao et al. [1], Han et al. [2], and Tao and Han [4]. Just like conventional CFST columns, CFDST columns under service loads, in a building or in bridges, will also suffer the effects of creep and shrinkage of the in-filled concrete. n Corresponding author. Tel.: þ86 10 62797067; fax: þ 86 10 62781488. E-mail address: lhhan@tsinghua.edu.cn (L.-H. Han). 0263-8231/$ - see front matter & 2011 Elsevier Ltd. All rights reserved. doi:10.1016/j.tws.2011.08.001 In the past, experiments on CFST columns under long-term sustained loading condition were reported by Nakai et al. [5], Terrey et al. [6], Morino et al. [7], Uy [8], Ichinose et al. [9], Han and Yang [10], Han et al. [11], Kwon et al. [12,13], and Yang et al. [14]. However, it appears that little attention has been given to the influence of longterm sustained loading on the behaviour of the CFDST columns, which indicates a need for further research in this area. The present study is an attempt to study the behaviour of CFDST column under long-term sustained loading. The purposes of this research are fourfolds. First, to report a series of tests to investigate the behaviour of CFDST columns under long-term sustained loading. Second, to develop numerical models on analysis to account for long-term sustained loading effects on CFDST columns. Third, to perform an analysis to investigate the long-term behaviour of CFDST columns using the numerical model. Finally, to develop a simplified formula for estimating the ultimate strength of CFDST columns subjected to long-term sustained loading. 2. Experimental programming 2.1. Specimens preparations Six tests, including two circular CFDST specimens as shown in Fig. 1(a), two square CFDST specimens as shown in Fig. 1(b), and two reference conventional CFST specimens, under concentrically sustained long-term sustained load were carried out. These specimens were tested under two stages, including the long-term service testing and ultimate load testing. In addition, ten CFDST L.-H. Han et al. / Thin-Walled Structures 49 (2011) 1534–1543 Nomenclature Aso Acn Bo Di Do fsyo fsyi fcu L M Mu N NL Nu NuL cross-sectional area of outer steel tube nominal concrete cross-sectional area inside the outer steel tube overall width of outer square steel tube overall diameter of inner circular steel tube overall diameter of outer circular steel tube steel yield strength of outer tube steel yield strength of inner tube concrete cube strength effective buckling length of column in the plane of bending bending moment ultimate bending strength of composite column at short-term loading condition axial load long-term sustained load ultimate strength of the composite columns at shortterm sustained loading condition ultimate strength of the composite columns at longterm sustained loading condition and CFST reference specimens without experiencing long-term sustained loading were also tested to measure their ultimate loads for comparison purposes. The outer steel tubes of all tested specimens have a sectional size of Do(Bo) to ¼120 1.96 mm, whilst the size of the inner Nuc Nue n t 1535 predicted ultimate strength experimental ultimate strength long-term sustained load level ð ¼ NL =Nu Þ reference time (in days) age at loading (in days) wall thickness of outer steel tube wall thickness of inner steel tube nominal steel ratio of CFDST ð ¼ Aso =Acn Þ stress strain instant strain at loading time long-term strain of concrete due to creep and shrinkage ð ¼ ecr þ esh Þ total strain creep component of strain shrinkage component of strain slenderness ratio ( ¼L/i, i is radius of gyration of crosssectional area) hollow ratio ð ¼ Di =ðDo 2to ÞÞ and Di =ðBo 2to Þ for circular and square CFDST columns, respectively t0 to ti an s e ei eL eo ecr esh l w steel tube is Di ti ¼60 1.96 mm. A summary of the specimens is presented in Table 1, where L is the length of the specimen; t is the sustaining time for long-term sustained loading; NL is the long-term sustained load; and n is the long-term sustained load level, and can be determined as n¼NL/Nu, where Nu is the Outer steel tube Sandwiched concrete to to ti Di ti Di Outer steel tube Inner steel tube Sandwiched concrete Inner steel tube Bo Do Fig. 1. Cross sections of CFDST: (a) circular section and (b) square section Table 1 Information of the testing specimens. Sectional type Number Specimen label Do(Bo) to (mm mm) Di ti (mm mm) L (mm) t (day) l fcu (MPa) w NL (kN) n Nue (kN) Nuc (kN) Circular 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 DC-1 DC-2 DCc-0n DCc-1 DCc-2 C-1 Cc-1 Cc-2 DS-1 DS-2 DSc-0n DSc-1 DSc-2 S-1 Sc-1 Sc-2 120 1.96 120 1.96 120 1.96 120 1.96 120 1.96 120 1.96 120 1.96 120 1.96 120 1.96 120 1.96 120 1.96 120 1.96 120 1.96 120 1.96 120 1.96 120 1.96 60 1.96 60 1.96 60 1.96 60 1.96 60 1.96 – – 1324 1324 1324 1324 1324 1200 1200 1200 1500 1500 1500 1500 1500 1386 1386 1386 1050 1050 – – – 1050 – – 1050 1050 – – – 1050 – – 40 40 40 40 40 40 40 40 40 40 40 40 40 40 40 40 66.4 66.4 39.3 66.4 66.4 66.4 66.4 66.4 66.4 66.4 39.3 66.4 66.4 66.4 66.4 66.4 0.52 0.52 0.52 0.52 0.52 0 0 0 0.52 0.52 0.52 0.52 0.52 0 0 0 177 354 – – – 305 – – 183 365 – – – 368 – – 0.3 0.6 – – – 0.6 – – 0.3 0.6 – – – 0.6 – – 779.1 836.9 578.0 789.9 715.4 796.7 878.1 835.0 1151.5 1042.7 800.0 1185.8 1135.8 1110.3 1116.2 1149.5 631.7 627.8 – – – – – – 898.6 891.3 – – – – – – Square n Ultimate test conducted at a concrete age of 28 days 60 1.96 60 1.96 60 1.96 60 1.96 60 1.96 – – – 1536 L.-H. Han et al. / Thin-Walled Structures 49 (2011) 1534–1543 ultimate strength of the CFDST columns at the short-term loading condition, which can be calculated using the method presented by Zhao et al. [1]. In Table 1, specimen designations starting with DC, DS, C, and S represent that the specimens are circular CFDST, square CFDST, circular CFST, and square CFST, respectively. A following letter c refers to their counterpart specimens, which were only tested under short-term loading. Two reference CFDST specimens were tested at a concrete curing age of 28 days, which are marked with stars in Table 1. Four sheet plates were cut, tack welded into a square shape, and then welded with a single bevel butt weld along the corners to form the square tube. One sheet plate was cut, rolled to a circular shape, and then welded with a single bevel butt weld for the circular tube. Each specimen was welded to a 25 mm thick steel base plate at the top and the bottom. Self-consolidating concrete (SCC) was used and filled into the gap between the outer and inner tubes without vibration. The SCC mix proportions by mass were as follows: cement:blast furnace slag:water:sand:coarse aggregate:additional high-range water reducer ¼300:200:181:994:720:3.6 (kg/m3). The fresh properties of the SCC mixture were given as follows: slump flow (mm): 270; concrete temperature (1C): 20; flow time (s): 13; flow speed (mm/s): 62; and flow distance (mm): 640. 2.2. Material properties The yield strength (fsyo) and the elastic modulus (Es) of the outer steel tubes for both circular and square CFDST specimens are 311 MPa and 205,500 N/mm2, respectively; the yield strength (fsyi) and the elastic modulus (Es) of the inner steel tubes are 380 MPa and 206,000 N/mm2, respectively. The material properties of the steel tubes for the CFST specimens are the same as those of the outer steel tubes for the CFDST specimens. The elastic modulus (Ec) of the sandwiched concrete at 28 days and at the time of ultimate load tests are 33,010 N/mm2 and 31,080 N/mm2, respectively, whilst the corresponding average cube strength (fcu) are 39.3 MPa and 66.4 MPa, respectively. 2.3. Experimental methodology The long-term service load tests started at 28 days after concrete casting. Fig. 2(a) shows the test set-up for the long-term service load tests. The long-term sustained load (NL) was applied by pre-stressing bars and controlled by means of a load cell. The load was kept constant with adjustments of these bars during the measurement. The axial deformations of the specimen were obtained by the deformation transducers, whilst eight gauges were mounted on the tube surface at mid-height to record the axial and transverse strains of the outer steel tube, shown in Fig. 2(a). The long-term service load tests lasted for about three years (1050 days) and were conducted under the room temperature and humidity of the laboratory. At the completion of the long-term service load tests, all the specimens were removed from the long-term loading devices and tested to failure under axial compression. Eight reference specimens without long-term service load applied were also tested at Top plate Top plate Loading Deformation cell Deformation transducer Specimen Strain gauge Pre-stress bar Specimen transducer Strain gauge Strain gauge meter Deformation transducer Bottom plate Bottom plate Fig. 2. Photos of the test set-up: (a) Long-term service test and (b) load-deformation test L.-H. Han et al. / Thin-Walled Structures 49 (2011) 1534–1543 the same time, while two related specimens (DCc-0n and DSc-0n) were tested earlier at the concrete age of 28 days. All tests were performed on a 5000 kN capacity testing machine, as shown in Fig. 2(b). Strain gauges were used for each specimen to measure the longitudinal and transverse strains at the midheight. Displacement transducers were used to measure the axial deformation and the lateral deflection. A load interval of less than one-tenth of the estimated load capacity was used. Each load interval level was maintained for about 2 min. 2.4. Test results and discussions 2.4.1. Long-term service test Fig. 3 shows the axial strain (eo) versus sustaining time (t) relationship for all tested specimens. It was found that, under the long-term sustained loads, eo increased significantly at the preliminary stage, and eo at 1 month attained approximately 60% of that at 4 months. After that eo developed much slower, and tended to stabilise after about 100 days. The trend of the longterm deformation for CFDST specimens was generally similar as that for CFST specimens. 750 600 450 300 Measured Predicted(FBM) Predicted(FEM) 150 formed (as shown in Fig. 4(b)), whilst the inner steel tube showed the inward buckling at the same region (as shown in Fig. 4(c)). The ultimate strengths (Nue) of all tested specimens are summarised in Table 1. It was found that Nue of the specimens DCc-0n and DSc-0n, which were tested at the concrete age of 28 days, is lower than that of the specimens tested after the longterm service load tests, due to the fact that concrete strength increased with the increase in its age. Fig. 5 shows the effect of long-term sustained loading on the load-bearing capacity of the tested specimens, where the non-dimensionalized ordinate bL is the ratio between the measured ultimate strengths of the member either experiencing long-term sustained loading or not. It can be found from Table 1 and Fig. 5 that, for CFST specimens, the load-bearing capacity of the specimens subjected to long-term sustained loads was slightly lower than that of the specimens without long-term sustained loads. For CFDST specimens, there is no obvious trend for the influence of the long-term sustained loading on the ultimate strength. Fig. 6 presents the axial load (N) versus lateral deflection (um) at mid-height relationship of the specimens under ultimate strength tests. It is found that, in general, the sustained longterm sustained load has a moderate effect on the shape of N–um relationship of both the CFST and CFDST specimens. 3. Numerical model Two types of numerical models, i.e. finite element model (FEM) and fibre-based model (FBM), were developed in this paper Axial strain, ε o (με) Axial strain, ε o (με) 2.4.2. Ultimate strength test After the ultimate strength tests, both the CFDST and CFST members exhibited an obvious overall buckling deformation, and the long-term sustained load had no obvious influence on the failure mode of columns. Fig. 4(a) shows the typical failure mode of CFDST specimen. It was found that the sandwiched concrete was crushed at the place where the outward buckling of outer steel tube was 750 600 450 300 Measured Predicted(FBM) Predicted(FEM) 150 0 0 0 300 600 900 0 1200 300 1500 900 1200 1500 Axial strain, ε ο (με) Axial strain, ε ο (με) 600 Time, t (day) Time, t (day) 1200 900 600 Measured Predicted(FBM) Predicted(FEM) 300 1200 900 600 Measured Predicted(FBM) Predicted(FEM) 300 0 0 0 300 600 900 1200 0 300 600 900 1200 Time, t (day) Time, t (day) 1500 Axial strain, ε ο (με) 1500 Axial strain, ε ο (με) 1537 1200 900 600 Measured Predicted(FBM) Predicted(FEM) 300 0 1200 900 600 Measured Predicted(FBM) Predicted(FEM) 300 0 0 300 600 900 Time, t (day) 1200 0 300 600 900 1200 Time, t (day) Fig. 3. Axial strain (eo) versus time (t) relationship. (a) DC-1 (n¼ 0.3), (b) DS-1 (n ¼0.3), (c) DC-2 (n ¼0.6), (d) DS-2 (n¼ 0.6), (e) C-1 (n¼ 0.6) and (f) S-1 (n¼ 0.6) 1538 L.-H. Han et al. / Thin-Walled Structures 49 (2011) 1534–1543 Crushed concrete Overall buckling Outward buckling of outer tube Inward buckling of inner tube Fig. 4. Typical failure mode of tested specimen (DC-2): (a) failure appearance, (b) sandwiched concrete and (c) inner steel tube 1.25 βL 1 0.75 0.5 0.25 S-1 C-1 DS-2 DS-1 DC-2 DC-1 0 Specimen label An 1/4 finite element model (FEM) was used herein for the purpose of saving calculation expense. The boundary conditions of the finite element model are shown in Fig. 7, where 1 represents the compressive loading; 2 denotes that the displacement of XY place is restrainted in the X direction; 3 denotes the symmetrisation against YZ plane (displacements of the concrete and end plate in the X direction, and displacements and rotations of the outer and inner tubes in the X direction are restrainted); 4 denotes symmetrisation against XY plane (displacements of the concrete in the Z direction, and displacements and rotations of the outer and inner tubes in the Z direction are restrainted); and 5 represents the rigid end plate. Fig. 5. bL of tested specimens. to predict the behaviour of the CFDST column subjected to longterm sustained loading. The FEM is more convenient for the detailed mechanism analysis of the CFDST than the FBM, however it costs more calculation expense than the FEM at the same time. Thus the FEM and FBM were used for the different analysis purposes, i.e. the FEM was used to carry out a detailed stress and strain analysis to reveal the long-term behaviour of the CFDST column, whilst the FBM was used to conduct parametric studies in this paper. 3.1. Finite element model (FEM) 3.1.1. General description ABAQUS 6.5 [15] software package was adopted for the finite element analysis. The steel tube was simulated using 4-node shell elements with reduced integration (S4R). The sandwiched concrete was modelled using 8-node brick elements (C3D8R), with three translation degrees of freedom at each node. A mesh convergence study was performed to identify an appropriate mesh density to achieve reliable results with reasonable computation times. Taking circular CFDST as an example, the adopted finite element mesh is shown in Fig. 7. The contact pressure model and the Coulomb friction model were adopted herein to simulate the normal and tangential surfaces behaviour between the steel tube and concrete, respectively [16]. Residual stress in the welded steel tubes was also included in the finite element model, using the method introduced by Han et al. [16]. 3.1.2. Material properties Elastic–plastic model was used to describe the constitutive behaviour of steel. A stress versus strain relation, which consists of five stages as shown by Han et al. [16], was adopted. Under the serviceability-level loading, the stress level of the core concrete in a CFST column generally remains in elastic stage [17]. The force redistribution caused by the long-term sustained loading effect of the concrete tends to transfer some external force originally resisted by the concrete to the steel tubes, resulting in a decrease of the concrete stress under the long-term sustained loading. Therefore, it is reasonable to use the viscoelasticity constitutive model herein to simulate the concrete material with the time effect considered [18,19]. While the stress relaxation behaviour is considered, the stress (sij) of a viscoelastic body can be demonstrated as follows [19]: Z t @ e ðt Þ sij ðtÞ ¼ dij lekk ðtÞ c1 ðtt0 Þ kk 0 dt0 @t0 0 Z t @e t0 ðÞ c2 ðtt0 Þ ij dt0 ð2Þ þ 2Geij ðtÞ @t0 0 where t is the referent time; t0 is the age at loading; dij is the Kronecker Delta (dij ¼1, if i¼j; and dij ¼0, if iaj); l and G are the material variables; c1(t) and c2(t) are the relaxation functions corresponding to volume strain ekk(t) and shear strain eij(t), respectively. l, G, c1(t) and c2(t) can be expressed as l ¼ Eðt0 Þ2Gðt0 Þ= 1þ fu , G ¼ Gðt0 Þ=1 þ fu , c1 ðtÞ ¼ ðfu =1 þ fu Þ½Eðt0 Þ2Gðt0 Þeht , c2 ðtÞ ¼ 2ðfu =1 þ fu ÞGðt0 Þeht , in which E(t0) and G(t0) are the elastic and the shear modulus, respectively, when sustained load is 1000 1500 800 1200 N (kN) N (kN) L.-H. Han et al. / Thin-Walled Structures 49 (2011) 1534–1543 600 400 DC-1 DCc-1 DCc-2 Predicted(FBM) Predicted(FEM) 200 0 0 10 20 30 DS-1 DSc-1 DSc-2 Predicted(FBM) Predicted(FEM) 900 600 300 40 0 50 0 10 1000 1500 800 1200 600 DC-2 DCc-1 DCc-2 Predicted(FBM) Predicted(FEM) 200 0 0 10 20 30 900 50 300 40 0 50 0 10 20 30 40 50 um (mm) 1500 800 1200 N (kN) N (kN) 40 600 1000 600 C-1 Cc-1 Cc-2 Predicted(FBM) Predicted(FEM) 200 30 DS-2 DSc-1 DSc-2 Predicted(FBM) Predicted(FEM) um (mm) 400 20 um (mm) N (kN) N (kN) um (mm) 400 1539 S-1 Sc-1 Sc-2 Predicted(FBM) Predicted(FEM) 900 600 300 0 0 0 10 20 30 40 0 50 um (mm) 10 20 30 40 50 um (mm) Fig. 6. Axial load (N) versus lateral deflection (um) relationship: (a) DC-1 (n¼ 0.3), (b) DS-1 (n¼0.3), (c) DC-2 (n¼ 0.6), (d) DS-2 (n¼0.6), (e) C-1 (n¼ 0.6) and (f) S-1 (n ¼0.6) element model [20]. The main function of the material subroutine program (UMAT) was to calculate the Jacobian matrix of the material constitutive model. The damage plasticity model was used to define the concrete material behaviour in the ultimate strength analysis with longterm effect considered. In the model, an equivalent stress–strain model proposed by Han et al. [16] was employed to simulate the plastic behaviour of the sandwiched concrete in CFDST under compression, by assuming that the inner tube can restrain the inner indentation of the concrete core, so the sandwiched concrete in the annulus is confined in the same way as that in a fully in-filled steel tube. It should be pointed out that the confinement factor (x), in the material model of Han et al. [16] was defined as follows for CFDST: x¼ Fig. 7. Finite element model of CFDST column. applied; h¼(1þ fu)k, k¼0.02; and fu is defined as the final creep coefficient. Similar to that of the normal CFST, fu ¼0.9 was adopted in this paper for the analysis of CFDST column under long-term sustained loading [20]. Using the visco-elasticity concrete model described above, a material subroutine program (UMAT) was developed in finite Aso fsyo fsyo ¼ an Acn fck fck ð3Þ in which Aso ¼ p½D2o ðDo 2to Þ2 =4 (for circular section) or B2o ðBo 2to Þ2 (for square section) is the cross-sectional area of the outer steel tube; Acn ¼ pðDo 2to Þ2 =4 (for circular section) or ðBo 2to Þ2 (for square section) is the nominal concrete crosssectional area inside the outer steel tube; fsyo is the yield stress of the outer steel tube, and fck is the compression strength of the concrete (the value of fck is determined using 67% of the cubic compression strength (fcu) in this paper); an ð ¼ Aso =Acn Þ is the 1540 L.-H. Han et al. / Thin-Walled Structures 49 (2011) 1534–1543 nominal steel ratio, which can reflect the effects of diameter (width)-to-thickness ratio ðDo ðBo Þ=to Þ of the outer steel tube, similar to that of the diameter(width)-to-thickness ratio of the steel tube in CFST columns [1,21]. Since long-term sustained loading effects need to be accounted for, the concrete model under short-term loading was modified. The method presented in Chu et al. [22] was used, which assumed that long-term sustained loading would not affect the concrete stress (s) but only change its strain (e). Fig. 8 shows the modified stress (s) versus strain (e) diagram at any time (t–t0) under a sustained stress st0, applied at time t0. After long-term strain (et ¼[1 þ f(t,t0)]et0 þ esh, in which f(t,t0) is creep coefficient, t andt0 are the sustaining time of the long-term sustained loading and the concrete age at loading, respectively, et0 is the corresponding short-term strain, and esh is shrinkage strain, which can be calculated using equations listed in Han [17]) being determined in the long-term service step, concrete stress versus strain relation in ultimate strength analysis can be defined by changing the short-term strain (et0) to the long-term strain (et) for considering the long-term effects [17], as shown in Fig. 8. 3.2. Fibre based method (FBM) In the past, the fibre based models (FBM), for predicting the long-term behaviour of the CFST column, had been established by Han and Yang [10] and Han et al. [11]. The FBM model was used herein to predict the long-term behaviour of CFDST columns under long-term sustained loading. The sectional element divisions for circular and square CFDST are shown in Fig. 9(a) and (b), respectively. As mentioned above, the sandwiched concrete of the CFDST columns in the annulus can be assumed to be confined in the same way as that in a fully in-filled steel tube, the material model for concrete of CFST, which was presented in Han and Yang [10], was used herein for the analysis of CFDST members. The confinement σ ε0 [1+ ϕ (t, τ 0 )] ε 0 + ε sh Long-term σ0 στ0 Short-term 0 ετ0 [1+ ϕ (t, τ 0 )] ε τ0 + ε sh factor (x), in the material model of Han and Yang [10], was defined as Eq. (3) for CFDST. 3.3. Verifications of the models The predicted time-history of axial strain (eo) under sustained loading by the finite element model (FEM) and the fibre based model (FBM) described above were compared with the current test results, as shown in Fig. 3. In addition, Fig. 6 shows the comparisons of axial load (N) versus lateral deflection (um) relationship for the current tests between the predicted and the test results. It can be seen that reasonably good agreements were obtained between the predicted and the test results. 4. Analytical behaviours Using the FEM described above, a detailed analysis on the longterm behaviour of CFDST columns was performed. A typical circular column, as shown in Fig.1(a), was selected to conduct the analysis. The calculating parameters of the member are Do ¼600 mm, an ¼0.1, w ¼0.5, Di/ti ¼60, l ¼40, fsyo ¼fsyi ¼345 MPa, fcu ¼60 MPa, n¼0.6, t0 ¼28 days, t¼50 years, and e/r¼0.5, where l ¼L/i is the slenderness ratio (i is radius of gyration of crosssectional area), and e/r is the load eccentricity ratio (e is the load eccentricity; r¼Do/2 is the radius of outer steel tube). For comparison purposes, a circular CFST column under long-term sustained loading was also calculated. The CFST column had a steel ratio (a ¼As/Ac, where As and Ac are the cross-section area of steel tube and concrete core, respectively) of 0.1, and had the same steel and concrete strength, load eccentricity ratio, and slenderness ratio(l) with those of the CFDST column mentioned above. 4.1. Load versus deflection response Fig. 10 shows the axial load (N) versus lateral deflection (um) at mid-height relationship for typical CFDST member with longterm sustained loading effect considered. Two characteristic points are marked on the curve, in which point A is corresponding to the beginning of sustained loading applied, and point B is the moment at the end of sustained loading applied. Meanwhile, Fig. 10 also gives the axial load (N), carried by the sandwiched concrete, outer steel tube, and inner steel tube of CFDST column subjected to long-term sustained loading versus lateral deflection (um) at mid-height relationship. As can be seen that during the long-term sustained loading stage (AB), the load of the CFDST member is kept stable. During this stage, due to the effect of long-term sustained loading, the lateral deflection of the CFDST column at mid-height tends to ε 10000 CFDST Fig. 8. Stress (s) versus strain (e) diagram of concrete. Outer steel tube Sandwiched concrete Inner steel tube Inner steel tube Sandwiched concrete N (kN) 8000 6000 A B Sandwiched concrete 4000 Outer steel tube Inner steel tube 2000 0 Outer steel tube Fig. 9. Schematic view of element division: (a) circular section and (b) square section 0 30 60 90 120 um (mm) Fig. 10. Axial load (N) versus lateral deflection (um) relationship. L.-H. Han et al. / Thin-Walled Structures 49 (2011) 1534–1543 increase. Since some external force carried by the concrete is transferred to the steel tubes, the deformation compatibility between the concrete and the steel tubes tends to result in the decrease of the concrete stress. The force carried by the sandwiched concrete is reduced by 30.5% during the long-term loading stage, whilst the loads on both the outer steel tube and inner steel tube increase each as 31.2%. Compared with the CFDST column, the reduction of the force carried by the core concrete in the CFST column is less significant with a proportion of 25%, whilst the loading increase of its outer steel tube is around 40.6%, which is bigger than that of CFDST column. This is due to the fact that, for the CFDST member, the inner steel tube could carry load transferred from the concrete. After the long-term sustained loading is finished and the compressive loading is applied, the lateral deflection at midheight keeps increasing. The axial load carried by the outer steel tube attains the peak point before the ultimate strength of the column is reached. After that, the force on the sandwiched concrete still keeps on increasing due to the confinement provided by the outer steel tube. The load carried by the inner steel tube keeps on increasing during the whole loading process. Fig. 11 shows the comparison of the axial load (N) versus lateral deflection (um) at mid-height relationship between the members with long-term sustained loading effect considered or not for the CFDST column. It can be found that the long-term sustained loading effects tend to decrease the ultimate strength of the composite column whilst increase the corresponding deflection. Once again, this contributes to the fact that the deformation during the long-term sustained loading stage tends to generate an additional moment to the CFDST column under compressive loading. This effect will cause a reduction of the ultimate strength as well as the improvement of the corresponding displacement. Compared with the CFDST column, the long-term sustained loading effects on the ultimate strength and the corresponding 10000 6000 4000 Long-term 2000 Short-term 0 0 30 60 90 120 um (mm) Fig. 11. Typical N–um relationship. deformation are more significant for the CFST column. For CFDST column experiencing long-term sustained loading, the ultimate strength decreases by 10.6% and the corresponding mid-height displacement increases by 7% compared with the member without long-term sustained loading effects considered, whilst those for the typical CFST are 11.5% and 15.9%, respectively. This contributes to the fact that, compared with the CFST column, the inner steel tube of CFDST can carry the compressive load together with the outer steel tube and their sandwiched concrete, which can lead to a lower compressive stress level in the concrete, and thus can decrease the influences of the long-term sustained loading on the behaviour of the CFDST column. 4.2. Interactive stress The interaction stresses p1 and p2 versus lateral deflection (um) relationship is shown in Fig. 12, in which p1 is the interaction stress between the outer steel tube and sandwiched concrete (point a), and p2 is that between the sandwiched concrete and the inner steel tube (point b). In Fig. 12, p 40 means that the interaction is present and p r0 indicates the occurrence of a separation tendency between the surfaces. The lateral deflection corresponding to the ultimate strength is also shown in the figure, where umu and umu’not are the lateral deflections with and without the consideration of the long-term sustained loading effect, respectively. It can be found from Fig. 12(a) that, due to larger Poisson’s ratio for steel at the initial loading stage, the lateral deformation of the steel tube is larger than that of the concrete, resulting in a separating trend between the outer steel tube and the sandwiched concrete. With the increase in the lateral deflection (um), the concrete begins to crack and its plasticity tends to develop as well. As a result, the lateral deformation of the concrete begins to exceed that of the steel tube, and the outer steel tube can provide the confinement for the concrete, thus resulting in an increase of the interaction stress p1 between them. Compared with the CFDST column under short-term loading, the long-term sustained loading effect tends to delay the occurrence of the interaction between the outer steel tube and the sandwiched concrete, as shown in Fig. 12(a). This is due to the fact that the decrease of concrete stress caused by the long-term sustained loading effect would delay the occurrence of the cracks in the concrete. The interaction stress p1 of the CFDST column with long-term sustained loading effect considered has not occurred until the ultimate strength is reached, and p1 of the specimen under short-term loading is approximately 3 MPa at this time, as shown in Fig. 12(a). Compared with the interaction stress p1, the interaction stress p2 is much smaller. Fig. 12(b) shows the comparison of the 2 8 Long-term Short-term a u 1 6 u p2 (MPa) p1 (MPa) N (kN) 8000 1541 u 4 a u b b 0 -1 2 Long-term Short-term -2 0 0 30 60 u m (mm) 90 120 0 30 60 90 um (mm) Fig. 12. Interactive stress (p) versus lateral deflection (um) relationship: (a) p1 and (b) p2 120 1542 L.-H. Han et al. / Thin-Walled Structures 49 (2011) 1534–1543 interaction stress p2 between the CFDST columns with or without considering long-term sustained loading effect. As can be seen the effects of long-term sustained loading on the interaction between the sandwiched concrete and the inner steel tube are moderate. 5. Parametric analysis and simplified model 5.1. Important parameters on the column strength Parametric analysis was performed to study the influence of different parameters on the ultimate strength of CFDST column under long-term sustained loading. The basic calculating condition is similar to the CFDST column shown in Section 4 of this paper. Fig. 13 gives a schematic view of load (N) versus mid-span lateral deflection (um) relationship of CFDST column with long-term sustained loading effects considered or not. It can be seen that the ultimate strength of a CFDST column under long-term sustained loading (NuL) is lower than that under short-term loading (Nu). Parametric analysis presented in this section is performed using the fibre element method (FBM). Fig. 14 illustrates the calculated interaction relationships between compressive strength ratio (N/Nu) and bending strength ratio (M/Mu) of the CFDST columns under different column slenderness ratio (l) with long-term sustained loading effect considered or not. It can be seen that the ultimate strength of the column with long-term sustained loading effects considered decreases compared with that of the column only under short-term loading, and the maximum strength reduction is around 30%. For convenience of analysis, strength index SI is defined to quantify the influencing of long-term sustained loading on the composite columns. It is expressed as SI ¼ NuL Nu ð4Þ where NuL is the ultimate strength with long-term sustained loading effects considered, and Nu is the ultimate load under short-term loading condition (as shown in Fig. 13). Influences of the changing slenderness ratio (l) and nominal steel ratio (an), strength of steel and concrete, concrete age (t0) at sustained loading, diameter-to-thickness ratio (Di/ti) of inner tube, long-term sustained load level (n), hollow ratio (w), and load eccentric ratio (e/r) on the ultimate strength of the CFDST members with long-term sustained loading effects considered were analysed. The range of these parameters are w ¼0–0.75, fsyo ¼235–420 MPa, fsyi ¼235–420 MPa, fcu ¼30–90 MPa, e/r¼ 0–1, an ¼0.05 0.2, n ¼0.2–0.8, Di/ti ¼30–90, and l ¼20–160. The results of parametric analysis showed that the effects of changing slenderness ratio (l), nominal steel ratio (an), strength of the outer tube steel (fsyo), strength of concrete (fcu), concrete age (t0) at sustained loading, long-term sustained load level (n), and load eccentric ratio (e/r) on the ratio of SI of CFDST columns were generally similar to those on SI of CFST columns, which had been previously presented in Han and Yang [10] and Han et al. [11]. The influence of the other parameters of CFDST, i.e. the yielding strength (fsyi) and the diameter-to-thickness ratio (Di/ti) of the inner steel tube as well as the hollow ratio (w) on SI, is shown in Figs.15, 16, and 17, respectively. It can be found from Figs.15 and 16 that the change of fsyi and Di/ti has a moderate influence on SI. However, SI increases with the increasing w, as shown in Fig. 17. This contributes to the fact that bigger w means 1.2 N fsyi=235MPa Short-term Strength index, SI 1.1 Nu NuL Long-term NL fsyi=345MPa 1.0 fsyi=390MPa 0.9 f syi =420MPa 0.8 0.7 0.6 0 O umL umo 80 120 160 200 Slenderness ratio, λ um umoL 40 Fig. 15. Influence of inner tube steel strength (fsyi). 1.2 1.0 Short-term Long-term 0.8 λ=20 λ=40 0.6 0.4 D /t =30 1.1 Strength index, SI Compressive strength ratio, N /Nu Fig. 13. Typical axial load (N) versus deflection (um) relationship. λ=80 0.2 D /t =60 1.0 D /t =90 0.9 0.8 0.7 λ=120 0.0 0.0 0.2 0.6 0.4 0.6 0.8 1.0 Bending strength ratio, M /Mu Fig. 14. N/Nu versus M/Mu relationship. 1.2 0 40 80 120 160 200 Slenderness ratio, λ Fig. 16. Influence of diameter-to-thickness ratio (Di/ti). L.-H. Han et al. / Thin-Walled Structures 49 (2011) 1534–1543 the outer and inner steel tubes. The long-term sustained loading effects on the ultimate strength and corresponding deformation of the CFST and CFDST members were generally similar. (3) The influences of changing steel strength and diameter-tothickness ratio of inner tube on the strength index (SICFDST) of CFDST columns subjected to long-term sustained loading were moderate, However, SICFDST increases with the increasing hollow ratio (w). (4) Formula for the calculations of the ultimate strength of CFDST columns subjected to long-term sustained loading was suggested in this paper, and the accuracy of the predictions is reasonable and somewhat conservative. 1.2 χ =0.25 Strength index, SI 1.1 χ =0.50 1.0 χ =0.75 0.9 0.8 0.7 0.6 0 40 80 120 160 Slenderness ratio, λ 1543 200 Acknowledgements Fig. 17. Influence of hollow ratio (w). a smaller cross-section area of the sandwiched concrete of CFDST, thus causing the influence of long-term sustained loading to be less significant. The research reported in the paper is part of the National Basic Research Program of China (973 Programme) (No.2009CB623200), and Tsinghua University Research Funds (No. 2010THZ02-1). The financial supports are highly appreciated. 5.2. Simplified model References Based on the results of parameter studies, the ultimate strength of CFDST columns after experiencing long-term sustained loading can be obtained by revising the formulas for CFST columns, where a factor of kw is multiplied to the strength index SI of CFST columns (SICFST), which had been proposed by Han [17], in order to consider the influence of hollow ratio (w). The expression of kw is suggested as follows using regression method based on the parametric analysis mentioned above, i.e. kw ¼ 0:65w2 0:45w þ 1 ð5Þ The strength index SICFDST simplified formulas for calculating the ultimate strength of CFDST columns with long-term sustained loading effects considered can be expressed as follows: SICFDST ¼ kw SICFST r 1 ð6Þ Using Eqs. (4)–(6), the ultimate strength of CFDST columns with long-term sustained loading effect considered can be expressed NuL ¼ SICFDST Nu ð7Þ The validity limits of Eq. (7) are: w ¼0–0.75, fsyo ¼235– 420 MPa, fsyi ¼235–420 MPa, fcu ¼ 30–90 MPa, e/r ¼0–1, an ¼ 0.05 0.2, n ¼0.2–0.8, Di/ti ¼ 30–90, l ¼20–160. The ultimate strength calculated with Eq. (7) is listed in Table 1, in which Nuc (¼SICFDST Nu, where Nu was calculated using the method presented by Zhao et al. [1]) is the predicted ultimate strength using the simplified formula. It can be found that the accuracy of the predictions is reasonable and somewhat conservative. 6. Conclusions The following conclusions can be made based on the limited research reported in the paper: (1) Long-term deformation of CFDST columns increases relatively fast at an early stage, whilst the process tends to stabilise after about 100 days. (2) Long-term sustained loading decreases the ultimate strength of the CFDST column whilst increases the corresponding deformation. During the long-term sustained loading stage, the force carried by the sandwiched concrete is transferred to [1] Zhao XL, Han LH, Lu H. Concrete-filled Tubular Members and Connections. Taylor & Francis: Spon Press; 2010. [2] Han LH, Tao Z, Huang H, Zhao XL. Concrete-filled double skin (SHS outer and CHS inner) steel tubular beam-columns. Thin-Walled Structures 2004;42(9):1329–55. [3] Tao Z, Han LH, Zhao XL. Behaviour of concrete-filled double skin (CHS inner and CHS outer) steel tubular stub columns and beam-columns. Journal of Constructional Steel Research 2004;60(8):1129–58. [4] Tao Z, Han LH. Behaviour of concrete-filled double skin rectangular steel tubular beam–columns. Journal of Constructional Steel Research 2006;62(7):631–46. [5] Nakai H, Kurita A, Ichinose LH. An experimental study on creep of concrete filled steel Pipes. In: Proceedings of the Third International Conference of ASCCS, Fukuoka, Japan; 1991: pp. 55–60. [6] Terrey PJ, Bradford MA, Gilbert RI. Creep and shrinkage of concrete in concrete-filled circular steel tubes. In: Proceedings of the Sixth International Symposium on Tubular Structures, Melbourne, Australia; 1994; pp. 293–8. [7] Morino S, Kswanguchi J, Cao ZS. Creep behavior of concrete filled steel tubular members. In: Proceedings of an Engineering Foundation Conference on steelconcrete composite structure, ASCE, Irsee, Germany; 1996; pp. 514–25. [8] Uy B. Static long-term effects in short concrete-filled steel box columns under sustained loading. ACI Structural Journal 2001;98(1):96–104. [9] Ichinose LH, Watanabe E, Nakai H. An experimental study on creep of concrete filled steel pipes. Journal of Constructional Steel Research 2001;57(4):453–66. [10] Han LH, Yang YF. Analysis of thin-walled steel RHS columns filled with concrete under long-term sustained loads. Thin-Walled Structures 2003;41(9):849–70. [11] Han LH, Tao Z, Liu W. Effects of sustained load on concrete-filled hollow structural steel columns. Journal of Structural Engineering, ASCE 2004;130(9):1392–404. [12] Kwon SH, Kim TH, Kim YY, Kim JK. Long-term behaviour of square concretefilled steel tubular columns under axial service loads. Magazine of Concrete Research 2007;59(1):53–68. [13] Kwon SH, Kim YY, Kim JK. Long-term behaviour under axial service loads of circular columns made from concrete filled steel tubes. Magazine of Concrete Research 2005;57(2):87–99. [14] Yang YF, Han LH, Wu X. Concrete shrinkage and creep in recycled aggregate concrete-filled steel tubes. Advances in Structural Engineering 2008;11(4):383–96. [15] Hibbitt, Karlson & Sorensen Inc. ABAQUS/standard user’s manual: Version 6.5. Providence, RI, USA; 2005. [16] Han LH, Yao GH, Tao Z. Performance of concrete-filled thin-walled steel tubes under pure torsion. Thin-Walled Structures 2007;45(1):24–36. [17] Han LH. Concrete filled steel tubular structures. Second edition Beijing: China Science Press; 2007. [in Chinese]. [18] Christensen RM. Theory of Viscoelasticity. Second edition New York: Academic Press; 1982. [19] Yang TQ, Luo WB, Xu P, Wei YT, Gang QG. Viscoelasticity theory and application. Beijing: China Science Press; 2004. [in Chinese]. [20] Li YJ. Effects of long-term sustained loads on the behavior of concrete filled steel tubular columns. Ph.D. thesis, Fuzhou University; 2009 [in Chinese]. [21] Bradford MA, Loh HY, Uy B. Slenderness limits for filled circular steel tubes. Journal of Constructional Steel Research 2002;58(2):243–52. [22] Chu KH, Domingo J, Carreira DJ. Time-dependent cyclic deflections in R/C beams. Journal of Structural Engineering, ASCE 1986;112(5):943–59.
0
You can add this document to your study collection(s)
Sign in Available only to authorized usersYou can add this document to your saved list
Sign in Available only to authorized users(For complaints, use another form )