POLYMERS FOR ADVANCED TECHNOLOGIES Polym. Adv. Technol. 2008; 19: 1276–1285 Published online 2 May 2008 in Wiley InterScience (www.interscience.wiley.com) DOI: 10.1002/pat.1124 Polyacrylamide-based material for electrospun humidity-resistant, water-soluble nanofilters Alexandre A. Vetcher1y, Ryan Gearheart1 and Victor N. Morozov1,2* 1 2 The National Center for Biodefense and Infectious Diseases, George Mason University, Manassas, VA 20110, USA Institute of Theoretical and Experimental Biophysics, Russian Acad. Sci, Pushchino, Moscow, 142290, Russia Received 16 January 2008; Accepted 21 February 2008 A new approach for the collection of aerosol particles is described in which the particles are first collected on a water-soluble filter and then liberated into an aqueous solution. The filter was manufactured by electrospinning a polyacrylamide (PAA) gel solution containing 2,2(-(bisacrylamino) diethyl disulfide (BAC) cross-links after gel dissolution in a water solution of b-mercaptoethanol. The morphology of the P(AA–BAC) nanofibers was characterized using atomic force microscopy (AFM) and optical microscopy. The filters were characterized for their ability to capture aerosol particles, their stability at high humidity, and their ability to release captured particles. Copyright # 2008 John Wiley & Sons, Ltd. KEYWORDS: fibers; nanotechnology; gas permeation; filter; electrospinning INTRODUCTION Filtration is the most extensively employed technology for aerosol sampling. Its simplicity1–3 favorably distinguishes it from technologies based on the inertial principle, i.e. impactors, impingers, cyclones, and centrifuges.4,5 When compared with these methods, filtration has the advantage of being highly economic in energy consumption, which makes this method especially attractive in the design of small, light, portable, and battery-operated (i.e., ‘‘personal’’6) aerosol samplers. Filtration is also preferable for its retention of bioaerosol structure and function since the aerosol is not subjected to high energy or force.3,7,8 Since energy consumption during filtration depends largely on the flow resistance of the filter, it is important to keep this resistance low. Filters made from fibers of a sub-micron diameter show a significant decrease in air resistance.9,10 Sub-micron fibers can be readily fabricated via the electrospinning process (ESP), in which a polymer solution or a melt is slowly squeezed through a capillary to which a high voltage is applied.11–13 After depositing such nanofibers onto a porous and conductive substrate, excellent filters have been fabricated from nylon and other materials9,10,14,15 which were capable of holding all aerosol particles with a diameter, d > 1 mm. This is commonly accepted as the size of biohazardous aerosols in many publications.6,16–18 Bioaerosols captured on a nanofilter must be released into an aqueous solution for further analysis (immunochemical, PCR, etc.). While the release of large water-insoluble particles may be accomplished efficiently,19 *Correspondence to: V. N. Morozov, The National Center for Biodefense and Infectious Diseases, George Mason University, Manassas, VA 20110, USA. E-mail: vmorozov@gmu.edu y Present address: Alcyon Bio, Inc., Germantown, MD 20874, USA. particles made from water-soluble biomaterials like toxins can be irreversibly adsorbed onto the filter during this procedure.20 An obvious solution to this problem consists in dissolution of filter with a solvent retaining viability and immunogenic properties of the collected biomaterial. Such an approach was first suggested in 1888 by Sedwick and Tornton21 who used granulated sugar to collect airborne germs from the air. Later soluble filters were prepared from alginate22 and from gelatin.23 The latter are now manufactured by SKC Inc. (Eighty-Four, Pennsylvania) and distributed by Sartorius. A major drawback of all these filters is in severe restrictions on air humidity.21,22,24 Here, we propose a new approach that combines the efficiency of bioaerosol collection via filtration with easy liberation of the collected material into a small volume of water-based solvent for subsequent immunoassay as schematized in Fig. 1. This new approach allows the manufacture of humidity-resistant filters which are soluble in aqueous solutions not harmful to biomaterials (Fig. 1A). It is based on the use of a cross-linkable polymer which can be uncrosslinked under mild conditions (Fig. 1C) after filtering the aerosol (Fig. 1B). We will demonstrate that a co-polymer of acrylamide (AA) with 2,20 -(bisacrylamino) diethyl disulfide (BAC)—previously used to liberate proteins and nucleic acids after electrophoresis25 —may be used as such a polymer material. EXPERIMENTAL Materials The following reagents were purchased from Sigma– Aldrich: ethanol (EtOH), dimethyl sulfoxide (DMSO), N,N-dimethylformamide (DMF), ethyl acetate (EtAc), acetic acid (CH3COOH), hydrochloric acid (HCl, (36.5–38%)), 2-mercaptoethanol (2-MET), Triton X-100, N,N,N0 ,N0 Copyright # 2008 John Wiley & Sons, Ltd. Polyacrylamide-based material for electrospun nanofilters 1277 Determination of disulfide and sulfhydryl (thiol) groups The well-known reaction of free thiols with DTNB26 was employed to estimate the content of thiol groups in the gel and fibers. To determine disulfide groups, the reactions were performed after the reduction of disulfides27 using NaBH4. The extinction coefficient for the DTNB product with thiol was taken as 12,800 1400 M1 cm1 according to the manufacturer’s recommendation. Before the determination of thiols and disulfides, nanomats were incubated at room temperature overnight. Gels were precipitated and washed 3–5 times with 100% EtOH for 60 min and then dried as described.28 Gel samples with a dry weight of 0.1–1.2 mg were taken for measurements of sulfhydryl and disulfide groups. Determination of zero shear viscosity Viscosity was measured with a home-made capillary viscometer at different flow rates and the zero shear viscosity was determined as described.29,30 The specific zero shear viscosity (hsp) was determined as hsp ¼ Figure 1. Schematic illustrating (A) the manufacture of a water-soluble nanofilter by the electrospinning–neutralization technique; (B) aerosol collection with such a filter; and (C) release of captured aerosol particles by breaking disulfide links in an aqueous reducing solution. This figure is available in colour online at www.interscience.wiley.com/journal/pat tetramethylethylenediamine (TEMED), AA, ammonium acetate (NH4CH3COO), DL-dithiothreitol (DTT), selenocystamine dihydrochloride (SCS), BAC, octyl b-D-glucopyranoside (OGP), ammonium persulfate (APS), sodium borohydride (NaBH4), polyvinylpyrrolidone (PVP) (MW 360 kDa), and 5,50 -dithiobis(2-nitrobenzoic) acid (DTNB). Nitrocellulose (NC) was purchased as parlodion strips from Electron Microscopy Sciences, Inc. (Hatfield, PA). Preparation of P(AA–BAC) gel Gel (2.75% w/v; AA/BAC is 10:1 w/w, or 37:1 M) was prepared by polymerization for 60 min at room temperature in a 50 ml Falcon tube in a water solution according to ref.25 After completion of polymerization, three volumes of EtOH were added to coagulate the gel and remove unincorporated monomers. The coagulated gel was then washed five times with EtOH and dried. The final, dried P(AA–BAC) contained 85 5% of the initial (AA þ BAC) mass. We will later refer to this product as P(AA–BAC)w. Since BAC has low solubility in water25 we tried to increase its incorporation into the gel by polymerizing the gel in a DMF/water mixture (2:1), under otherwise similar experimental conditions. We will refer to this product as P(AA–BAC)d and use the abbreviation P(AA–BAC) when referring to both materials or to the material in general. The gels were dissolved overnight in a solution containing 10% 2-MET and 20% EtOH via slow rotation before placing them into the electrospinning apparatus. We shall refer to the latter solvent as ESS. Copyright # 2008 John Wiley & Sons, Ltd. hs h0 h0 (1) where hs and h0 are the zero shear viscosities of solution and solvent, respectively. Ultrasound treatment Freshly dissolved 5% P(AA–BAC) solutions in ESS were placed in 2 ml Eppendorf tubes and treated with ultrasound at 22.5 kHz by a horn sonicator (Microson XL-2000 from Misonix, Inc., Farmingdale, NY). The temperature increase resulting from this treatment was controlled with a thermocouple and not allowed to rise above 378C. As a reference, 1 g of P(AA–BAC)w was treated as described above without dissolution in ESS. Gel swelling measurements Several gels were tested for swelling: (i) initial P(AA–BAC)w gel precipitated in EtOH and dried as described above, (ii) P(AA–BAC)w gel treated with ultrasound for 10 sec at 30 W and then dried, (iii) P(AA–BAC)w gel dissolved in ESS and then dried on a glass surface, and (iv) P(AA–BAC)w gel dissolved in ESS, treated with ultrasound, and then dried on a glass surface. Drying occurred at þ608C for 24 hr, and ultrasound treatment was performed for 10 sec at 30 W. Five pieces of each dried gel sample with masses of 4–32 mg were kept for 24 hr at room temperature in 10 ml of water. Excess water was removed by aspiration and the weight of swollen gel, Wh, was determined. The water intake was characterized by the swelling ratio28,31,32: S¼ Wh Wd Wd (2) where Wd is the dry weight of the gel. The standard deviation in measurements of S was estimated as 10%. Fabrication of nanofilters by electrospinning ESP has been conducted in a device shown schematically in Fig. 1A. In contrast to conventional fabrication techniques which use conducting substrates, in this technology Polym. Adv. Technol. 2008; 19: 1276–1285 DOI: 10.1002/pat 1278 A. A. Vetcher, R. Gearheart and V. N. Morozov nanofibers are neutralized with a cloud of counter-ions generated via electrospray.29,33 Such in-air-neutralization results in the manufacture of free nanomats and nanomats on a dielectric mesh substrate. The same conditions were used in the manufacture of all of the nanofilter samples: (i) neutralizing liquid—absolute EtOH; (ii) distance between neutralizing capillary tip and target—12 cm, (iii) distance between spinneret and the target—15 cm, (iv) voltage— positive 18 kV at the spinneret, (v) current 0.45 0.1 mA, (vi) flow rate of polymer solution—2 ml/min, and (vii) humidity in chamber 22–40%. ESP was conducted on an adjacently arranged glass slide (Fisherbrand plain microscope slide Fisher Scientific Corp. (Pittsburgh, PA) cleaned in plasma discharge) and on a polyester mesh, 105 mm (CMY-0105, obtained from Small Parts, Inc, Miami Lakes, FL) until a visible spot appeared. PVP was electrospun from an 8% solution in EtOH, while NC was electrospun from a 12.7% solution in EtAc. Optical microscopy was conducted using an inverted Axiovert-25 microscope from Carl Zeiss, GmbH (Jena, Germany) with 40 magnification. Images were captured with a Pixera digital camera employing version 3.0 of Viewfinder software (Pixera Corp., Los Gatos, CA). Atomic force microscopy (AFM) was performed using a Nano-R AFM instrument from Pacific Nanotechnology, Inc. (Santa Clara, CA). Images were made in the tapping mode under dry conditions created by passing a weak stream of air dried over silica-gel. All measurements were made using Femtoscan Online v. 2.2.71 software (obtained from Moscow State University and Advanced Technologies Center, Moscow, Russia). Design of the filter unit A piece of mesh supporting a nanomat was glued to the cut-and-buffed end of a plastic tube with a 6 mm ID using an epoxy glue, as shown schematically in Fig. 1. The actual working area was smaller than this due to the glue. The open filter area was determined by acquiring an optical image of the filter surface and calculating the open filter area using the SCION-NIH program, which is freely available on the Internet. The working filter area was found to be 82 8% of the total internal tube area. Filter resistance to air flow was measured as follows. A filter was connected to a pump in such a way as to have the nanomat pulled against the mesh surface under working conditions. The volumetric flow rate (Q) was measured with a digital flow meter (32707-34 from Cole Parmer Instrument Comp., Vernon Hills, IL). The pressure drop on the filter (P) was measured with a digital manometer (Sper Scientific, Ltd., Scottsdale, AZ). For each resistance measurement, the dependence of Q on P was plotted within the interval of volumetric flow rates from 0.5 to 5 l/min. Permeability to gas flow was characterized by the apparent Darcy flow resistance coefficient,9,14,15,34 RD: RD ¼ AP mQ (3) where A is the area of test sample, and m is the dynamic air viscosity. Copyright # 2008 John Wiley & Sons, Ltd. It was shown in several independent measurements using the same filter that the standard deviation in determining the Q(P) slope did not exceed 2%.Total error in the calculated RD due to this error and the uncertainty in A was estimated as 3–5%. In all the measurements no deviation of Q(P) from a linear relationship was detected in the flow rate interval tested. Generation of aerosol Aerosol was generated in a closed 125 l plastic chamber, using two techniques. In the first technique, a soot aerosol was generated by a burning candle.35 In the second technique, polystyrene fluorescent particles with a diameter of 0.87 0.02 mm (Spherotech Inc, Lake Forest, IL) were aerosolized from an aqueous 0.01% suspension using an ultrasonic nebulizer (Zewa Inc., Miami, FL). Single fluorescent particles were seen deposited on filters after such a nebulizing procedure. The humidity inside the chamber was adjusted by the evaporation of water from filter paper and measured with a digital hygrometer (Sper Scientific, Ltd., Scottsdale, AZ). To ensure a uniform distribution of humidity and aerosol, air inside the chamber was stirred with a fan. Determination of aerosol filtration ability The aerosol capture efficiency of filters was determined by counting soot aerosols of different sizes (0.3–0.5, 0.5–0.7, 0.7–1, 1–2, 2–5, and >1 mm) passed through the filter using a laser particle counter (ParticleScan, Pro IQAir North America, Inc., Santa Fe Springs, CA). The particle counter was connected to the chamber via two silicon tubes (6 mm ID) of equal lengths. Two solenoid-operated valves allowed the pumping of air from the aerosol-containing chamber into the counter either via the control channel, which contained only a multi-turn needle valve, or through the channel containing the filter. Before measurement, volumetric flow rates in the two channels were equalized using the needle valve. Because the aerosol concentration was slowly changed over time, a series of measurements were quickly made first for the control channel, then for the filter, and then again for the control. The retention (filtration) efficiency9 was calculated as 2RF % (4) E ¼ 100 1 RC1 þ RC2 where RC1 and RC2 are counter readings in the control channel before and after reading in the filter channel, respectively. RF is the reading in the filter channel. After switching channels, we allowed the pipeline to be filled with a new sample of aerosol, starting measurements only when the last count differed from the previous one by no more than the Poisson’s scatter for the given level of counting. With the entire cycle taking 3 min, the average difference between RC1 and RC2 was found to be 2.5 2.7%. Thus, aerosol aggregation did not affect our retention measurements substantially. Retention of nano-aerosols was determined at a flow rate of 0.3 l/min using a TSI aerosol analyzer (CPC 3781 equipped with CPMS 3085, kindly provided by TSI Incorporated Polym. Adv. Technol. 2008; 19: 1276–1285 DOI: 10.1002/pat Polyacrylamide-based material for electrospun nanofilters (Shoreview, MN)) by comparing spectra of nano-aerosol particles in the laboratory air with those in the air passed through the filter. Humidity resistance under low pressure was estimated in two experiments. In the first test, the filter was kept in a humidity chamber with 100% humidity. After storage in the chamber, filters were inspected under an optical microscope for changes in their morphology; afterwards, E and RD were determined. In the second experiment, the humidity of air in the aerosol chamber was raised by the evaporation of water and aerosol was then collected from wet air. Changes in E and RD were continuously monitored during collection. After aerosol collection, filter morphology was inspected, again using optical microscopy. Humidity resistance under high pressure A special device was designed to characterize the strength of filters in humid air. The filter holder was designed as a unit that could be placed under a microscope to visually monitor changes in the filter while recording them with a digital camera. Tubing was used to connect the holder to a 45 l plastic bag filled with air. The bag was directly attached to a plastic chamber equipped with a fan, a humidity meter, and inlets and outlets for the introduction of humid air, etc. Before the experiment, dry air was removed via vacuum and humid air was pumped into the bag. To adjust air humidity, either the air was bubbled through water or a measured amount of water was introduced into the chamber and allowed to evaporate. This was performed until the desired relative humidity was achieved. The air was then forced to pass through the filter by a vacuum pump connected to the filter outlet. The pressure drop on the filter was continuously measured by a differential digital manometer. Aerosol releasing ability measurements After collection, aerosolized fluorescent particles were first counted directly on the filter under a fluorescent microscope. The filter was then treated with a solvent and the particles were counted again. The efficiency of each solvent was determined by averaging the data of at least three parallel experiments. 1279 the wash solution (20 mM Tris-HCl, 0.15 M NaCl, and 0.05% Tween-20, pH 7.5). Afterwards, 150 ml of pNPP was added to each well and OD readings at 405 nm were taken after 5, 10, 20, and 40 min of incubation with shaking. RESULTS AND DISCUSSION Choice of dissolution (decomposition) agents The schematic in Fig. 1 presents the major steps in manufacturing water-soluble cross-linkable nanofilters, their use in capturing aerosol particles, and their dissolution with the liberation of captured particles. Different properties are required in the solvent used for the preparation of the P(AA–BAC) solution in nanofilter manufacture and in the solvents used in filter dissolution. In the first case, the reducing reagent should be volatile and non-conductive. These requirements exclude DTT and NaBH4 from consideration, leaving only 2-MET as a suitable reducing reagent and we determined that 10% 2-MET works quite well. It was also found that addition of 20% EtOH improves the electospinning process and does not precipitate the P(AA–BAC) solution. The most important feature of the solution to be used in the filter dissolution is non-interference with the chosen detection method (ELISA). This requirement excludes NaBH4 from consideration as it is a strong reducing agent, and leaves only 2-MET and DTT. We have chosen 10 mM DTT because it is effective at low concentrations and is a common component of many standard buffers. To facilitate DTT action, 1 mM SCS, a known catalyst of thiol–disulfide exchange reactions,36–38 was added to the solution as well as 0.2% Triton X-100. We will refer to this solvent as ARS. It was found that 50 ml of ARS completely dissolved a P(AA–BAC) nanomat, 6 mm in diameter, in 2 min. The effects of ARS and the filter degradation products on immunoassay were estimated using the direct ELISA protocol described in the Experimental section. As seen in Fig. 2, ELISAs performed in a solution containing ARS and Testing of filter dissolution products for their effects on ELISA Nunc MaxiSorp flat-bottomed, 96-well microtiter plates were first coated with ovalbumin (Ova). Fifty microliterof a 10 mg/ ml Ova solution in 50 mM sodium carbonate buffer, pH 9.5, were placed in each well and the 96-well plate was incubated for 1 hr at room temperature. The plate was then blocked with a blocking solution (1% BSA in 20 mM Tris-HCl, 0.15 M NaCl, and 0.05% Tween-20, pH 7.5) for 30 min and the wells were washed two times with the washing buffer. Serial dilutions of anti-Ova-IgG-AP conjugate were made in each of the following six solutions: (i) 1% BSA (as a standard), (ii) 10 mM DTT, (iii) 1 mM selenocystamine, (iv) 0.2% Triton X-100, (v) a combination of all of the above, and (vi) a solution of 0.02 mg of nanofibers dissolved in 20 ml of solution (v). The wells were incubated with these solutions at room temperature for 1 hr with shaking and then washed three times with Copyright # 2008 John Wiley & Sons, Ltd. Figure 2. Direct ELISA in the presence of P(AA–BAC) dissolution components. The solution components tested were: (^) 10 mM DTT, (&)1 mM selenocystamine, (~) 0.2% Triton X-100, (^) all of the above components (ARS), (&) 0.02 mg of P(AA–BAC) nanomat dissolved in 20 ml of ARS, (~) standard blocking solution (20 mM TRIS/HCl, pH ¼ 7.5, 0.15 M NaCl, 1% BSA, 0.1% Tween-20). Color intensity was measured after a 40 min incubation in pNPP solution. Polym. Adv. Technol. 2008; 19: 1276–1285 DOI: 10.1002/pat 1280 A. A. Vetcher, R. Gearheart and V. N. Morozov the dissolved P(AA–BAC) nanofilter retain approximately 70% of the ELISA signal in the standard buffer. Therefore, we conclude that a captured bioaerosol can be analyzed using standard immunoassay techniques. Optimization of ESP conditions for nanofilter manufacture Formation of thin fibers with good morphology is essential to the manufacture of effective filters. Despite great efforts to systematically study the factors which affect the ESP,11–13,39 the process remains something of an art. Nevertheless, certain factors must be kept in an appropriate range in order to fabricate fibers of sufficient quality. Solution viscosity (h) is one factor13,39 which greatly affects the fiber morphology.40,41 One known method of predicting electrospinnability and estimating nanofiber diameter and quality is based on the De Gennes’ scaling concept.42 This scaling law requires the construction of a logarithmic plot of the hsp of a polymer solution of a specified molecular weight against the concentration, C. The plot typically contains several areas with unique slopes. As the concentration passes from the semi-dilute, unentangled area (with hsp (C)1.25), to the semi-dilute, entangled area (with hsp (C)4.8), a notable change in the slope is observed at the concentration corresponding to the entanglement concentration, Ce (Fig. 3). Electrospinning of polymer solutions with concentrations greater than Ce results in the formation of fibers free of beads and other defects.41,43–51 If the gel is polymerized after removal of traces of dissolved gases from the solution by the barbotage of nitrogen, P(AA–BAC) does not dissolve in 10% 2-MET after Figure 3. Dependence of hsp on polymer concentration. (~) PAA (400 KDa) in water (ref.28), (~) P(AA–BAC) solution in 10% 2-MET and 20% EtOH treated with ultrasound. Arrows indicate the entanglement concentration Ce. Copyright # 2008 John Wiley & Sons, Ltd. overnight stirring. We attribute this observation to the ability of dissolved oxygen to act as a radical chain-breaker. Its removal results in polymer chains of sufficient length, so that even a small fraction of residual disulfide bonds are capable of maintaining the gel structure. In view of this, all other experiments were conducted using P(AA–BAC) gels polymerized without nitrogen barbotage. Upon dissolution of P(AA–BAC) in 2-MET, we noted that, although the P(AA–BAC) gel readily disintegrates, it does not turn into a homogeneous solution even after several days of slow stirring. This inhomogeneity became apparent when jellyfish-like incorporations were observed in the nanomat after electrospinning. We have identified these as mini-gels based on their microscopic appearance.52 The problem of solution inhomogeneity may be solved by a brief exposure to ultrasound. A significant reduction in the solution viscosity was observed as a result of this treatment, as illustrated in Fig. 4. We speculate that strong shear stress and/or cavitations break bonds in gel aggregates that remained in the dissolved P(AA–BAC). The average effective molecular weight of the P(AA–BAC) polymer in the ultrasound-treated solution was estimated by comparing the concentration dependence of viscosity of this solution to that of solutions of linear PAA polymers with known molecular masses.29 As one can see in Fig. 3, ultrasoundtreated P(AA–BAC) demonstrates a concentration dependence similar to that of linear PAA with a molecular weight of 400 kDa. In a separate experiment we determined that linear PAA has the same viscosity in water as in ARS. From the concentration dependence of viscosity, we estimated the entanglement concentration for the ultrasound-treated P(AA–BAC) as Ce 2.7%. The dependence of the normalized viscosity of PAA–BAC solutions on the sonication energy, presented in Fig. 4, demonstrates that the viscosity drops rapidly as a function of the dose, reaching a plateau at an energy of 100 J. This Figure 4. Dependence of normalized specific viscosity of solutions of linear PAA and P(AA–BAC) on sonication energy. (*) PAA (12 kDa), (~) PAA (22 kDa), (~) PAA (80 kDa), (*) PAA (400 kDa) and (^) PAA (5 MDa, sonicated at power 10 W), (^) 1% PAA (5 MDa sonicated at different powers for 10 sec); (&) 1% PAA (5 MDa sonicated at 10 W), (&) 4.5% P(AA–BAC) sonicated in a solution containing 10% 2-MET and 20% EtOH. Sonication was performed in a 2 ml Eppendorf tube at a power of 5 W, if not indicated otherwise, and 1 ml solution was sonicated. PAA solutions with concentration of 5% PAA were used if not indicated otherwise. Polym. Adv. Technol. 2008; 19: 1276–1285 DOI: 10.1002/pat Polyacrylamide-based material for electrospun nanofilters behavior is similar to the dependence of linear PAA with a MW of 5 MDa, which was shown29 to disintegrate to 1 MDa fragments after ultrasound treatment with a dose of 100 J. Based on the similarity in concentration dependence of ultrasound-treated P(AA–BAC) and ultrasound-treated linear PAA, we conclude that the presence of SH side groups does not notably increase entanglement in P(AA–BAC) solutions as compared to linear PAA of a similar molecular weight and concentration. 1281 Table 2. Swelling of different P(AA–BAC) gels in water (see Materials and Methods for details) Solvent for polymerization Dissolution in ESSa Ultrasound treatmentb Swelling ratio (S)c Water Water Water Water DMF/Water 2:1 þ þ þ þ þ þ 14.7 2d 7.5 0.6 8.8 0.9 25.1 2.4 37.8 4.3 a Thiol and disulfide groups in P(AA–BAC) To characterize the extent of cross-linking of P(AA–BAC) in gels and nanomats, we performed measurements of combined thiol and disulfide groups after gel polymerization and after ESP. Two different gel concentrations, 2.75 and 5.25%, with AA/BAC ratios of 20:1 and 10:1 w/w, respectively, were chosen. For polymerization in water we were unable to incorporate BAC at a ratio greater than 1:20 w/w or 1:80 M. Polymerization in DMF resulted in the incorporation of larger fractions of BAC: 1:16 w/w with the same starting 1:10 ratio. This can be explained by the higher solubility of BAC in DMF than in water. The amount of free thiols was negligible in the dried gel since all sulfur in BAC is in the disulfide form (Table 1). However, it is difficult to conclude how many of those are involved in inter-chain cross-links. Some BAC was not linked to the gel or belongs to chains not connected to the gel network: nanomats not washed in EtOH contained 77% more combined thiol and disulfide groups as compared to the initial P(AA–BAC) gels. Gel dissolution in 2-MET followed by drying the solution on a glass surface resulted in an 40% increase in the disulfide and thiol content, presumably due breaking BAC links and introduction of 2-MET into the gel. It follows from this interpretation that the number of intermolecular cross-links should drop dramatically after the dissolution of the original gel followed by drying. To further verify this, we estimated the change in the number of cross-links by measuring the swelling ratio in the original and restored gels since the number of cross-links determine the extent of swelling.28,53,54 Gel swelling The data on swelling of P(AA–BAC) gels are presented in Table 2. One can see that neither ultrasound treatment of the gel alone, followed by drying, nor its dissolution alone followed by drying, leads to an increase in the swelling ratio. In fact, the ratio decreases approximately two-fold, pre- Gels were dissolved to a concentration of 5% w/v. Ultrasound treatment was performed for 10 sec at a power of 30 W. c Average of five separate gel samples, 4–32 mg each, kept for 24 hr at room temperature in a large excess of water. d Average of 15 gel samples, 4–32 mg each, made from two gels. The samples were kept for 24 hr at room temperature in a large excess of water. b sumably due to the difference in the drying procedure (drying alone in the case of treated gels vs. precipitation with EtOH followed by drying in the case of the original gel). However, the combination of dissolution and ultrasound treatment resulted in a approximately two-fold increase in the swelling ratio, indicating fewer dense inter-molecular cross-links in the ‘‘restored’’ gels. We speculate that a significant shortening of the chains results in fewer cross-links and less entanglement of the chains. This makes gel swelling easier. Thus, dissolution of P(AA–BAC) in ESS with subsequent ultrasound treatment and evaporation of the solvent lead to the formation of a gel with a lower content of cross-links, as judged from the increased swelling of such a gel. Considering the fact that drying of the gels proceeded with a much lower rate as compared to that upon formation of nanofibers in ESP, we expect that the number of cross-links formed in the fibers is even lower than in the restored gel and hence they will be subjected to greater swelling. ESP conditions for P(AA–BAC) nanofibers The data presented in Fig. 5 clearly illustrate the previously discussed connection between entanglement of polymer molecules and nanofiber morphology. As expected, when the P(AA–BAC) concentration in the ultrasound-treated solution exceeds Ce ¼ 2.7%, (C/Ce 1 in Fig. 5) fibers which are free of beads predominate in the nanomat. The histogram of df distribution demonstrates a typical broad character.29,41,44,45,47,48 The dependence of the P(AA–BAC) fiber diameter on the concentration normalized to Ce is presented Table 1. Molar disulfide and thiol content in different P(AA–BAC) samples (in moles of sulfur per 100 moles of AA, see Experimental section for details) Sample no. Sample description 1 2 3 4 5 6 P(AA–BAC)w gel washed for 60 min in EtOH dried No. 1 dissolved in ESSa, dried for 24 hr at 608C Nanomat from no. 1 after ESP No. 3 washed for 100 min in 70% EtOH P(AA–BAC)d gel washed for 60 min in EtOH and dried No. 5 dissolved in ESS, dried for 24 hr at 608C a Thiolb Disulfideb 0.18 0.02 — 0.5 0.08 0.13 0.01 — — 3 0.1 3 0.3 5.3 0.9 3.2 0.3 4.1 0.2 4.2 0.5 Gels were dissolved to a concentration of 5% w/v. Average of three separate gel samples, 0.1–1.2 mg each. b Copyright # 2008 John Wiley & Sons, Ltd. Polym. Adv. Technol. 2008; 19: 1276–1285 DOI: 10.1002/pat 1282 A. A. Vetcher, R. Gearheart and V. N. Morozov Figure 5. Morphology of nanofibers spun from P(AA–BAC) solution in SSA. The method of observation (optical or AFM) is indicated below the figures while the concentration of the solution normalized to Ce is shown in the inset linking optical and AFM images belonging to the same sample. The right panels exhibit the distribution of nanofiber diameters which were measured as heights in AFM images. The length of the bar is 10 mm. in Fig. 6 and is described by the empirical formula: df ¼ a b C Ce (5) with the parameters: a ¼ 104 nm, b ¼ 1.2 and the coefficient of determination, R2 ¼ 0.93. This analysis led us to choose a Figure 6. Dependence of fiber heights on concentration normalized to Ce. All data were obtained in solution containing 10% 2-MET and 20% EtOH. Copyright # 2008 John Wiley & Sons, Ltd. minimal P(AA–BAC) concentration of C ¼ 5%, resulting in thin, defect-free fibers, which we further used for filter manufacture. Humidity resistance of P(AA–BAC) nanomats When P(AA–BAC) nanomats and nanomats made from water-soluble polymers (PVP-1M and PAA-5M) were placed in 100% humidity for 10 min, only P(AA–BAC) nanomats remained on the mesh as visually intact, while the other two disappeared entirely. Similarly, nanomats from watersoluble polymers disappeared after being breathed upon while those made of P(AA–BAC) survived a deep exhale (Fig. 7B), incubation at 100% humidity (Fig. 7C), and pumping through the filter a humid (95% humidity) air (Fig. 7D). No significant changes in either RD or E were seen in P(AA–BAC) nanomats stored at 100% humidity for 24 hr, as seen in Table 3. P(AA–BAC) nanofilters also demonstrated good stability in the dynamic humidity test. As shown in Table 3, the aerosol-capturing efficiency, E, decreased by 8 5% after Polym. Adv. Technol. 2008; 19: 1276–1285 DOI: 10.1002/pat Polyacrylamide-based material for electrospun nanofilters 1283 Figure 8. Retention of aerosol particles with a diameter exceeding 1 mm as a function of resistance to air flow for a series of nanofilters electrospun from different P(AA–BAC) concentrations normalized to Ce: (^) 1.67 mm, (&) 1.33 mm, (~) 1.17 mm, and (~) 1 mm. Figure 7. Optical images of P(AA–BAC) filters on a mesh before and after subjection to high humidity. (A) Filter not subjected to humidity. (B) Filter which was breathed on. (C) Filter after a 10 min incubation at 100% humidity at room temperature. (D) Filter after 10 min work with air at 95% humidity pumped through Bar denotes 50 mm. pumping humid air through the filter for 10 min. The observed increase in the resistance to air flow may be attributed to a mutual gluing of adjacent nanofibers. This is noticeable even in optical microscopy, as illustrated in Fig. 7D. Despite these changes, P(AA–BAC) nanofilters demonstrated good humidity resistance under even the harshest working conditions. Nanofilters manufactured from P(AA/BAC)d and PVP were subjected to increasing air pressure of varying humidity levels to determine the dependence of filter strength on humidity. The filters were subjected to humid air pressure for 10–15 min. It was found that the PVP nanofilter was effective up to 0.7 atm at a humidity less than 83%. When the humidity was increased to 87 2% and the pressure raised to 0.7 atm, however, 17% of the PVP filter surface was damaged within a few minutes. In contrast, no visible destruction was observed in the P(AA–BAC)d filters subjected to 0.5 atm at 97% humidity. Using the data presented in Fig. 8, one can estimate the minimal power requirement for filtration of air with a specified efficiency at a specified volumetric flow rate through the filter. Assuming that the volume of liquid used to elute the captured aerosol is 50 ml, we chose a filter area with a diameter of 6 mm. For a filter with RD of 108 m1 Figure 9. Spectra of sub-micron aerosol particles in laboratory air (filled circles) and in the air passed through a humidity-resistant soluble (P(AA–BAC) nanofilter (open circles). A filter with an area of 0.16 cm2 is characterized by a resistance to air flow, RD ¼ 1 108 m1. working at a pressure of 0.5 atm, one can filter 40 l/min by a battery-operated device consuming only 5 mW. Aerosol capturing efficiency The aerosol filtration efficiency of P(AA–BAC)-based nanofilters has been determined for particles of different sizes. Comparisons of E for aerosols of different sizes were routinely used to check the filter integrity: filters which showed E < 100% independent of size were considered as having macro-holes and discarded. Figure 8 illustrates the parametric dependence of filtration efficiency, E, on RD for a number of filters manufactured from different P(AA–BAC) concentrations and different deposition times. In general, the Table 3. Effect of passive exposure to a humid environment and effect of filtering humid air on resistance of P(AA–BAC) nanofilters to air flow and on their ability to capture aerosol particles Normalized to initial valuea (%) Treatment Incubation at 100% humidity for 60 min Incubation at 100% humidity for 24 hr Collection of aerosol at 95 1% humidity for 10 min Range of examined RD (107 m1) RD E for particles with d >1 mm 0.82–1.53 0.82–1.53 1–19.3 93 11 87 11 165 20 81 8 69 17 93 5 a Normalization was performed according to the equation (Vf/Vi) 100%, where Vi is the measured value before treatment and Vf is the value after treatment. Nanomats were electrospun from 4.5% P(AA–BAC) in ESS. Copyright # 2008 John Wiley & Sons, Ltd. Polym. Adv. Technol. 2008; 19: 1276–1285 DOI: 10.1002/pat 1284 A. A. Vetcher, R. Gearheart and V. N. Morozov Table 4. Comparison of P(AA–BAC) and SKC gelatin filtersa (SKC Inc., Eighty-Four, Pennsylvania) Property Capturing efficiency for 1 mm aerosol Resistance to air flow, RD 107 m1 Maximum humidity Minimum humidity Dissolving conditions Minimum volume of solvent for a filter, 25 mm in diameter SKC filter, 3 mm P(AA–BAC) filter >96% 120 85% Short work-time to avoid drying 378C, buffer solution 5 ml 80–90 1–2 100% No Buffer solution with DTT or 2-MET 0.1 ml a Data for the SKC filters (catalog no. 225–9551) are taken from web site: http://www.skcgulfcoast.com/products/featuredproducts.asp?catno¼225–9551 and from ref.55 dependence of E on RD is similar to that reported for nanomats made of electrospun nylon and other polymers.9,10,14,15 Using an opportunity to test a TSI aerosol analyzer manufactured by TSI Incorporated (Shoreview, MN), we analyzed the efficiency of P(AA–BAC) nanofilters in capturing nano-aerosol particles. As one can see in Fig. 9, a filter with RD ¼ 1 108 m1 was able to capture 80% of all particles that were 100 nm in diameter, on average, and 5060% of particles that were 20–30 nm in diameter. We conclude, therefore, that such filters could be used not only for the collection of micron-sized aerosols but also for viral aerosols with the highest degree of dispersion—when aerosol particles contain single viruses. It is important to compare our P(AA/BAC) filters with the commercially available gelatin SKC filters, since the latter are widely used to collect cells and viruses for analysis. One can see from Table 4 that, unlike the SKC filters P(AA–BAC) filters provide much less resistance to air, do not have maximum and minimum working humidity, and can be dissolved in smaller solution volumes. Release of captured aerosol particles from P(AA–BAC) nanofilters After applying a droplet of ARS to a P(AA–BAC) filter for 0.5–1 min and collecting the liquid with Whatman paper, only occasional fluorescent beads were seen under a fluorescent microscope on the wet filter area (Table 5). We estimated that all the captured fluorescent particles had been quickly transferred into the ARS droplet. In contrast, only 50% of particles were released when P(AA–BAC) filters were washed with water. Similar data were obtained from water-insoluble NC nanofilters. Addition of detergent to water resulted in a slight increase in the removal of particles for both the filters tested. These data show that micron-sized aerosol particles can be removed from waterinsoluble filters by washing them with detergent solution. Table 5. Fraction of captured particles released from nanomats under different washing conditions Washing procedurea Nanomat Darcy composition coefficient 107 m1 NC PAA/BAC 1.12–4.98 0.75–10 Water 0.1% Triton X-100 49.2 5 56.3 24b 70 3 58.7 21b a The columns denote washing with 50 ml of water or 50 ml of 0.1% Triton X-100, respectively. b During the washing procedure the nanomat partially collapsed, burying some nanoparticles. Copyright # 2008 John Wiley & Sons, Ltd. However, water-soluble aerosols cannot be released with this simple technique due to their ability to adsorb on a large surface of fibers, and thus only water-soluble filters solve this problem. CONCLUDING REMARKS Nanofilters electrospun from oxidizable polymers containing free thiol residues combine good stability at high humidity with good solubility under mild conditions, retaining the majority of the structure and function of most macromolecules and living cells. We envisage multiple applications of these nanofilters in inexpensive aerosol collectors for testing microbes, pollen allergens, and toxins both indoors and outdoors as well as in devices which integrate aerosol collection and biosensor-based detection of specific pathogens or allergens. Acknowledgments The authors gratefully acknowledge support from DOE, grant DE-F C52-04NA25455. The authors are grateful to Mr. J. Baker for the opportunity to test the TSI instrument in our laboratory. We also acknowledge the valuable advice of Dr. Timothy Born concerning the manuscript. REFERENCES 1. Huang HL, Yang SH. Filtration characteristics of polysulfone membrane filters. J. Aerosol Sci. 2006; 37: 1198–1208. DOI:10.1016/j.jaerosci.2005.11.010 2. Lee KW, Mukund R. In Aerosol Measurements: Principles, Techniques and Application, Baron P, Willeke K (eds). John Wiley & Sons: NY, 2001; 197–228. 3. Crook B. In Bioaerosols Handbook, Cox CS, Wathes CM (eds). CRC Press LLC: Boca Raton, FL, 1995; 269–284. 4. Crook B. In Bioaerosols Handbook, Cox CS, Wathes CM (eds). CRC Press LLC: Boca Raton, FL, 1995; 247–268. 5. Marple VA, Olson BA, Rubow KL. In Aerosol Measurements: Principles, Techniques and Application, Baron P, Willeke K (eds). John Wiley&Sons: NY, 2001; 229–260. 6. Agranovski IE, Safatov AS, Borodulin AI, Pyankov OV, Petrishchenko VA, Sergeev AN, Sergeev AA, Agranovski V, Grinshpun SA. New personal sampler for viable airborne viruses: feasibility study. J. Aerosol Sci. 2005; 36: 609–617. DOI:10.1016/j.jaerosci.2004.11.014 7. Morris KJ. In Bioaerosols Handbook, Cox CS, Wathes CM (eds). CRC Press LLC: Boca Raton, FL, 1995; 285–316. 8. Lacey J, Venette J. In Bioaerosols Handbook, Cox CS, Wathes CM (eds). CRC Press LLC: Boca Raton, FL, 1995; 407–472. 9. Gibson P, Schreuder-Gibson H, Rivin D. Transport properties of porous membranes based on electrospun nanofibers. Colloids Surf. Physicochem. Eng. Asp. 2001; 187: 469–481. DOI:10.1016/S0927–7757(01)00616-1 10. Gibson P, Schreuder-Gibson H, Rivin D. Electrospun fiber mats: transport properties. Aiche J. 1999; 45: 190–195. DOI:10.1002/aic.690450116 Polym. Adv. Technol. 2008; 19: 1276–1285 DOI: 10.1002/pat Polyacrylamide-based material for electrospun nanofilters 11. Reneker DH, Chun I. Nanometre diameter fibres of polymer, produced by electrospinning. Nanotechnology 1996; 7: 216–223. DOI:10.1088/0957–4484/7/3/009 12. Subbiah T, Bhat GS, Tock RW, Pararneswaran S, Ramkumar SS. Electrospinning of nanofibers. J. Appl. Polym. Sci. 2005; 96: 557–569. DOI:10.1002/app.21481 13. Li D, Xia YN. Electrospinning of nanofibers: reinventing the wheel? Adv. Mater. 2004; 16: 1151–1170. DOI:10.1002/ adma.200400719 14. Schreuder-Gibson H, Gibson P, Senecal K, Sennett M, Walker J, Yeomans W, Ziegler D, Tsai PP. Protective textile materials based on electrospun nanofibers. J. Adv. Mater. 2002; 34: 44–55. 15. Schreuder-Gibson HL, Gibson P. Applications of electrospun nanofibers in current and future materials. Polym. Nanofibers 2006; 918: 121–136. 16. Agranovski V, Ristovski Z, Hargreaves M, Blackall PJ, Morawska L. Performance evaluation of the UVAPS: influence of physiological age of airborne bacteria and bacterial stress. J. Aerosol Sci. 2003; 34: 1711–1727. DOI:10.1016/S0021– 8502(03)00191-5 17. Agranovski V, Ristovski Z, Hargreaves M, Blackall PJ, Morawska L. Real-time measurement of bacterial aerosols with the UVAPS: performance evaluation. J. Aerosol Sci. 2003; 34: 301–317. DOI:10.1016/S0021–8502(02)00181-7 18. Agranovski V, Ristovski ZD. Real-time monitoring of viable bioaerosols: capability of the UVAPS to predict the amount of individual microorganisms in aerosol particles. J. Aerosol Sci. 2005; 36: 665–676. DOI:10.1016/j.jaerosci.2004.12.005 19. Gopal R, Kaur S, Feng CY, Chan C, Ramakrishna S, Tabe S, Matsuura T. Electrospun nanofibrous polysulfone membranes as pre-filters: Particulate removal. J. Memb. Sci. 2007; 289: 210–219. 20. Ryu JH, Lee E, Lim YB, Lee M. Carbohydrate-coated supramolecular structures: Transformation of nanofibers into spherical micelles triggered by guest encapsulation. J. Am. Chem. Soc. 2007; 129: 4808–4814. DOI:10.1021/ja070173p 21. Sternberg GM. A Text-Book of Bacteriology, William Wood and Co: NY, 1896. 22. Richards M. A water-soluble filter for trapping airborne micro-organisms. Nature 1955; 176: 559–560. DOI:10.1038/ 176559b0 23. Burton NC, Grinshpun SA, Reponen T. Physical collection efficiency of flter materials for bacteria and viruses. Ann. Occup. Hyg. 2007; 51: 143–151. 24. Salvador A, Chisvert A. An environmentally friendly (‘‘green’’) reversed-phase liquid chromatography method for UV filters determination in cosmetics. Anal. Chim. Acta, 2005; 537: 15–24. DOI:10.1016/j.aca.2004.12.047 25. Hansen JN. Electrophoresis of ribonucleic acid on a polyacrylamide gel which contains disulfide cross-linkages. Anal. Biochem. 1976; 76: 37–44. DOI:10.1016/0003–2697(76)90261-X 26. Ellman GL. A colorimetric method for determining low concentrations of mercaptans. Arch. Biochem. Biophys. 1958; 74: 443–450. DOI:10.1016/0003–9861(58)90014–6 27. Cavallini D, Graziani MT, Dupre S. Determination of disulphide groups in proteins. Nature 1966; 212: 294–295. DOI:10.1038/212294a0 28. Patras G, Qiao GG, Solomon DH. Characterization of the pore structure of aqueous three-dimensional polyacrylamide gels with a novel cross-linker. Electrophoresis 2000; 21: 3843–3850. DOI:10.1002/1522–2683(200011)21:17<3843:: AID-ELPS3843>3.0.CO;2-G 29. Vetcher AA, Gearheart R, Morozov VN. Correlation of morphology of electrospun fibers with rheology of linear polyacrylamide solution. Polym. J. 2007; 39: 878–881. DOI:10.1295/polymj.PJ2006269 30. Rudin A, Chee KK. Zero shear viscosities of narrow and broad distribution polystyrene melts. Macromolecules 1973; 6: 613–624. DOI:10.1021/ma60034a028 31. Nam K, Kimura T, Kishida A. Physical and biological properties of collagen-phospholipid polymer hybrid gels. Biomaterials 2007; 28: 3153–3162. DOI:10.1016/j.biomaterials.2007.03.001 32. Nam K, Kimura T, Kishida A. Preparation and characterization of cross-linked collagen-phospholipid polymer hybrid gels. Biomaterials 2007; 28: 1–8. DOI:10.1016/j.biomaterials.2006.08.002 33. Morozov VN, Vsevolodov NN. Electrospray-neutralization method for manufacturing free and supported nanomats. Adv. Funct. Mater. 2007; 19: 4381–4386. Copyright # 2008 John Wiley & Sons, Ltd. 1285 34. Darcy H. Les Fontaines Publiques de la Ville de Dijon, Dalmont: Paris, 1856. 35. Grinshpun SA, Adhikari A, Honda T, Kim KY, Toivola M, Rao KSR, Reponen T. Control of aerosol contaminants in indoor air: combining the particle concentration reduction with microbial inactivation. Environ. Sci. Technol. 2007; 41: 606–612. DOI:10.1021/es061373o 36. Chen Y, Maret W. Catalytic selenols couple the redox cycles of metallothionein and glutathione. Eur. J. Biochem. 2001; 268: 3346–3353. DOI:10.1046/j.1432-1327.2001.02250.x 37. Singh R, Kats L. Catalysis of reduction of disulfide by selenol. Analyt. Biochem. 1995; 232: 86–91. DOI:10.1006/ abio.1995.9956 38. Tsen CC, Tappel AL. 1958; Catalytic oxidation of glutathione and other sulfhydryl compounds by selenite. J. Biol. Chem. 1958; 233: 1230–1232. 39. Huang ZM, Zhang YZ, Kotaki M, Ramakrishna S. A review on polymer nanofibers by electrospinning and their applications in nanocomposites. Composites Sci. Technol. 2003; 63: 2223–2253. DOI:10.1016/S0266–3538(03)00178-7 40. Helgeson ME, Wagner NJ. A correlation for the diameter of electrospun polymer nanofibers. Aiche J. 2007; 53: 51–55. DOI:10.1002/aic.11056 41. Wang C, Hsu CH, Lin JH. Scaling laws in electrospinning of polystyrene solutions. Macromolecules 2006; 39: 7662–7672. DOI:10.1021/ma060866a 42. De Gennes PG. Scaling Concepts in Polymer Physics, Cornell University Press: Ithaca, NY, 1979. 43. Ohkawa K, Minato KI, Kumagai G, Hayashi S, Yamamoto H. Chitosan nanofiber. Biomacromolecules 2006; 7: 3291–3294. DOI:10.1021/bm0604395 44. McKee MG, Elkins CL, Long TE. Influence of selfcomplementary hydrogen bonding on solution rheology/ electrospinning relationships. Polymers 2004; 45: 8705–8715. DOI:10.1016/j.polymer.2004.10.049 45. McKee MG, Hunley MT, Layman JM, Long TE. Solution rheological behavior and electrospinning of cationic polyelectrolytes. Macromolecules 2006; 39: 575 583. DOI:10.1021/ ma051786u 46. McKee MG, Long TE. Implication of hydrogen bonding on rheological/electrospinning relationships. Abs. Pap. Am. Chem. Soc. 2004; 228: U376–U376. 47. McKee MG, Wilkes GL, Colby RH, Long TE. 2004; Correlations of solution rheology with electrospun fiber formation of linear and branched polyesters. Macromolecules 37: 1760–1767. DOI:10.1021/ma035689h 48. Gupta P, Elkins C, Long TE, Wilkes GL. Electrospinning of linear homopolymers of poly(methyl methacrylate): exploring relationships between fiber formation, viscosity, molecular weight and concentration in a good solvent. Polymers 2005; 46: 4799–4810. DOI:10.1016/j.polymer.2005.04.021 49. Shenoy SL, Bates WD, Frisch HL, Wnek GE. Role of chain entanglements on fiber formation during electrospinning of polymer solutions: good solvent, non-specific polymerpolymer interaction limit. Polymers 2005; 46: 3372–3384. DOI:10.1016/j.polymer.2005.03.011 50. Shenoy SL, Bates WD, Wnek GE. Correlations between electrospinnability and physical gelation. Polymers 2005; 46: 8990–9004. DOI:10.1016/j.polymer.2005.06.053 51. Tan SH, Inai R, Kotaki M, Ramakrishna S. Systematic parameter study for ultra-fine fiber fabrication via electrospinning process. Polymers 2005; 46: 6128–6134. 52. Kazakov S, Kaholek M, Kudasheva D, Teraoka I, Cowman MK, Levon K. Poly(N-isopropylacrylamide-co-1-vinylimidazole) hydrogel nanoparticles prepared and hydrophobically modified in liposome reactors: atomic force microscopy and dynamic light scattering study. Langmuir 2003; 19: 8086– 8093. DOI:10.1021/la030066i 53. Patras G, Qiao GG, Solomon DH. Controlled formation of microheterogeneous polymer networks: Influence of monomer reactivity on gel structure. Macromolecules 2001; 34: 6396–6401. DOI:10.1021/ma010484z 54. Patras G, Qiao GG, Solomon DH, Koch R. Synthesis, characterization, and modelling of novel multifunctional acryloylbased monomers: An experimental and computational study. Aust. J. Chem. 2002; 55: 675–680. DOI:10.1071/CH01082 55. Burton NC, Grishpun SA, Reponen T. Physical collection efficiency of filter materials for bacteria and viruses. Ann. Occup. Hyg. 2007; 51: 143–151. Polym. Adv. Technol. 2008; 19: 1276–1285 DOI: 10.1002/pat
0
You can add this document to your study collection(s)
Sign in Available only to authorized usersYou can add this document to your saved list
Sign in Available only to authorized users(For complaints, use another form )