Title: Hardness Testing
Group 5: Sam Pecoraro, Luke Muffitt, Spencer Rieman, Brendon Rickle
Date Performed: 9/5/2025, Date Report Submitted:
OBJECTIVES: The objective of these tests are to determine the hardness of five different materials,
1018 Steel, 1045 Steel, Ductile Cast Iron, 6061 Aluminum and A2 Tool Steel. The hardness of each
material will be tested on three scales, Brinell Hardness, Rockwell B Scale, and Rockwell 30T scale.
PROCEDURE: see appendix
RESULTS:
Steel is defined as an alloy of carbon and iron with a carbon content of less than 2%. Generally,
steels with a higher percentage of carbon content are harder. A2 has a carbon content of approximately
1%, 1045 has a carbon content of approximately 0.45%, and 1018 has a carbon content of approximately
0.18%. While ductile Iron contains carbon, the carbon forms in pockets of graphite during casting, as
opposed to carbides in steel. This difference makes ductile iron softer than steel. Aluminum is softer than
steel due to its crystalline structure, allowing the atoms to easily slide past each other.
The data from the tests was unexpected. According to the data, Ductile Iron was the second
hardest in 2 of the 3 hardness tests, with a Mean HRB of 93 and a relatively large standard deviation. In
theory, Ductile iron should be harder than aluminum, but not the other steels. Another surprise was 1045
having an HRB of 94, being harder than A2’s HRB of 92; based on the carbon content difference, A2
should’ve been harder. 6061 was expected to be the softest metal, and it was with an HRB of 57. The
larger variations, or standard deviation, could be caused by inconsistencies in the metals.
The conversions were done using a hardness conversion table. The data from the conversions
isn’t as accurate as the tested BHN. Some of the tested BHNs deviate from the converted BHNs
considerably; for instance, the HR30T-converted BHN for 6061 differed 19% from the tested BHN value.
This could be due to differences in precision between the Rockwell tester in the lab and the testers used to
create the chart, or most likely due to variations in surface hardness.
1045 had the lowest percent difference between tested and converted BHNs of the 5 metals. The
converted BHN from HRB was only 1.45% larger than the tested value, while the converted value for
HR30T was 3.38% smaller than the tested HRB.
APPENDIX - ADDITIONAL PAGES, STAPLED TO PAGE ONE (in the order shown):
HARDNESS MACHINE TEST PROCEDURE:
Measure the hardness of five materials supplied. Use both the Brinell and Rockwell testers for all
samples. Be sure to use the correct indenter for the Rockwell test and the correct load and dwell time for
the Brinell Test (refer to lecture notes if needed). Use both the B and 30T scales when doing the
Rockwell Test. Take three measurements using each Rockwell method.