Quick Welding Procedure
Base Material:
Alloy Designation:
Principal Composition:
P-Number:
Group No.:
SA-533 Gr. B
K12539
Mn–1Ú2Mo–1Ú2Ni
3
3
to: SA-517 Gr. B
K11630
1Ú2Cr–1Ú5Mo–V
11B
4
Preheat Temperature:
10 C (50 F) for t < 13 mm (1/2 in.). 121 C (250 F) for t > 13 mm or minimum tensile strength exceeding 410
Mpa (60 ksi)
Filler Wire (GTAW):
ER80S-D2
F-Number:
6
A-Number:
11
AWS:
5.28
Interpass temperature:
316 C (600 F) max. Not mentioned in ASME Sec. VIII Div. 1, taken from API 582
Electrode (SMAW):
E7018-A1
F-Number:
4
A-Number:
2
AWS:
5.5
Postweld Heat Treatment:
650 C (1200 F) for all thicknesses except for SA-202 Gr. A and B when (t) > 16 mm. Holding time for t ≤ 50
mm (2 in.) = 1hr/25 mm (1 in.); for t > 50 mm (2 in.) and t ≤ 125 mm (5 in.) 1 hr/25 mm (1 in.) and for t > 125
mm (5 in.), 5hr + 15min/25 mm (1 in.) for each additional 25 mm (1 in.) over 125 mm (5 in.). Minimum
holding time is 15 minutes.
General Comments:
This copy of WeldPulse® is licensed to PetroStreet