Ceramics International 50 (2024) 29632–29641
Contents lists available at ScienceDirect
Ceramics International
journal homepage: www.elsevier.com/locate/ceramint
Effects of grain boundary phase distributions on mechanical characteristics
of the high thermal conductivity AlN ceramics
Xin Wei a, Hao Zhang b, c, Junjie Dang b, c, Haixian Xu b, c, Jun Guo b, c, Jingwei Li a, Song Cui c, d,
Wenming Tang a, d, *
a
School of Materials Science and Engineering, Hefei University of Technology, Hefei, 230009, China
Hefei Shengda Electronic Technology Industry Co. Ltd., Hefei, 230088, China
43rd Institute, China Electronics Technology Group Corporation, Hefei, 230088, China
d
Anhui Province Key Laboratory of Microsystem, Hefei, 230088, China
b
c
A R T I C L E I N F O
A B S T R A C T
Handling Editor: Dr P. Vincenzini
AlN powders with different O impurity contents were used to fabricate the high thermal conductivity (TC) AlN
ceramics of different grain boundary (GB) phase distributions via pressureless sintering. Bending strength,
fracture toughness, R-curve characteristic, and fracture mechanism of the ceramics were then investigated. The
results showed that the GB phase distributions had great influences on mechanical characteristics of the ce­
ramics. The ceramics with the continuous/semi-continuous GB phases possessed low strength and toughness.
Comparatively, the ceramics with the isolated island-like GB phases, especially the fine GB phases at the triple
AlN GB junctions, owned higher strength and toughness. The AlN ceramics principally followed the intergranular
fracture mode, but the GB phase distribution had great effects on the fractions of transgranular fracture. The AlN
ceramics with the continuous/semi-continuous GB phases had a lower fraction of the transgranular fracture, and
thus lower crack propagation resistance and reliability than the others.
Keywords:
Sintering
Grain boundaries
Microstructure-final
Mechanical properties
1. Introduction
AlN ceramic has become an ideal substrate material for
manufacturing power semiconductor devices owing to its low coefficient
of thermal expansion (CTE), matchable properties with those of Si and
GaAs semiconductors (AlN: 4.2 × 10− 6/◦ C, Si and GaAs: 3–4 × 10− 6/
◦
C,25–200 ◦ C), low dielectric constant (1 MHz, 8.0) and dielectric loss,
high electrical insulation properties, and importantly the high thermal
conductivity (TC), theoretically 320 W/(m⋅K) [1–3]. Currently,
commercially available high-TC AlN ceramic substrates usually have
TCs of more than 200 W/(m⋅K). However, heat accumulation in an
in-service high-power semiconductor device preferentially generates
high thermal stress at the circuit connections [4,5], mainly inducing
crack expansion and even fracture of the ceramic substrates. In addition,
power semiconductor devices, especially those used in electric vehicles,
frequently suffer vibration and impact stresses. Therefore, the AlN
ceramic substrates of high strength and toughness are usually required
to guarantee the safety and reliability of the power semiconductor de­
vices and the material in ballistic scenarios [6,7] in addition to high-TC.
To date, researches on TC of the AlN ceramics and its affecting fac­
tors have been widely reported [8–11]. However, strength and tough­
ness of the AlN ceramics was ignored or rarely reported. Generally, the
strength and TC of the AlN ceramics both depend on the microstructural
factors of the ceramics, such as AlN grain size, content and distribution
of the GB phase, and porosity, in which the GB phase has the most sig­
nificant influence [12,13]. It is well known that Y2O3 is the most
commonly used sintering additive in preparation of the high-TC AlN
ceramic substrates [13,14]. During sintering the AlN ceramics, Y2O3
reacts with O impurities to form the Y–Al–O oxide melt, and then it
gradually crystallizes in the cooling process of the ceramics to form the
GB phases at the AlN GB such as YAG (Y3Al5O12), YAP (YAlO3), and
YAM (Y4Al2O9) [15–17]. The CTE of these GB phases is approximately
twice of that of AlN (AlN: 4.2 × 10− 6/◦ C, YAM: 7.8 × 10− 6/◦ C, and
Y2O3: 7.5 × 10− 6/◦ C, 25–200 ◦ C [15,18]) which induces residual ther­
mal stress at the GB phase/AlN interface and the adjacent AlN GBs. The
residual stress in the AlN ceramics is related to the GB phase distribu­
tions [15]. For example, a compressive stress at the AlN GBs is induced
by the adjacent isolated island-like GB phases [15], enhancing the GB
* Corresponding author. School of Materials Science and Engineering, Hefei University of Technology, Hefei, 230009, China.
E-mail address: wmtang@hfut.edu.cn (W. Tang).
https://doi.org/10.1016/j.ceramint.2024.05.260
Received 19 March 2024; Received in revised form 9 May 2024; Accepted 17 May 2024
Available online 18 May 2024
0272-8842/© 2024 Elsevier Ltd and Techna Group S.r.l. All rights are reserved, including those for text and data mining, AI training, and similar technologies.
X. Wei et al.
Ceramics International 50 (2024) 29632–29641
binding strength, and inhibiting crack propagation along the GBs. While
a tensile stress at the GB phase/AlN interface is evoked by the
continuous/semi-continuous GB phases [15], decreasing the GB binding
strength, and promoting crack propagation preferentially along the GBs.
As a result, the residual stress has great effects on the TC, strength,
toughness, and fracture mechanism of the AlN ceramics. Kilmera et al.
[19] reported that with the GB phase distribution in the AlN ceramics
changed from the continuous state to the isolated island-like state, the
TC and bending strength of the AlN ceramics apparently increased.
Suzuki et al. [20] reported that the AlN ceramics containing 0.5 wt%, 5
wt% Y2O3 sintering additives had different microstructures. In the AlN
ceramics containing 0.5 wt%Y2O3 sintering additive, the GB phases
appeared in the isolated islands-like state, and thus the transgranular
fracture of the AlN grains was preferred. However, in the AlN ceramics
containing 5 wt%Y2O3 sintering additive, the GB phases were in the
hybrid isolated island-like and continuously distributed state, and the
ceramics predominantly followed the intergranular fracture mode. Lee
et al. [21] prepared the AlN ceramics by adding 3 wt% of Y2O3 and 3 wt
% of CaZrO3 as the sintering additive, and then pressureless sintering
and heat treatment at 1600 ◦ C for 3 h and 1400 ◦ C for 2 h, successively.
The TC of the ceramics was 156 W/(m K) with the bending strength as
high as 560 MPa, mainly attributing to the distribution of the fine GB
phase at the triple AlN GB junctions. Baek et al. [22] developed the AlN
ceramics by adding 1 wt% of ZrO2 to the multi-component oxide sin­
tering additive and pressureless sintering at 1600 ◦ C for 1 h. The
resulting product had a low TC (109 W/(m⋅K)) but an extremely high
bending strength of 608 MPa. The formation of isolated island-like
Y–Al–O GB phase and ultrafine ZrN particles at the triple AlN GB junc­
tions reinforced the ceramics, and thus improved the crack propagation
resistance.
In the current authors’ previous research [23], the detailed study on
relationship between TC and microstructure of high-TC AlN ceramics
was executed. In this work, AlN powders with different O contents were
chosen as raw materials to prepare the high-TC AlN ceramic substrates
of different GB phase distributions. The AlN ceramics were fabricated
using advanced industrial technology for fabricating the AlN ceramic
substrates, including slurry preparation, tape casting, stacking,
degreasing, pressureless sintering, and heat treatment [23]. Further, the
investigation on bending strength, fracture toughness, R-curve charac­
teristic, and fracture mechanism of the AlN ceramics with different GB
phase distributions were then carried out. This study is believed to
provide supports for design and process optimization of the AlN ceramic
substrates of high TC, strength, toughness, and reliability for electronic
packaging in future.
2. Experimental
2.1. Processing
Three kinds of ultrafine AlN powders, named A, B, and C (Hefei
Shengda Electronic Technology Industry Co. Ltd., Hefei, China) with
different O contents were synthesized through the carbothermal
reduction nitridation process [24] at different N2 flow rates (150, 200,
250 L/min, respectively) with a holding time of 12 h at 1700 ◦ C.
Table 1
Characteristics of the AlN powders with different O contents.
(Table 1). The AlN powder was blended with 5 wt% of Y2O3 sintering
additive, and the AlN green bodies were prepared by ball milling and
mixing, casting, isostatic pressure molding, debinding and other pro­
cesses [23].
The AlN green bodies of different O contents were pressureless sin­
tered in a graphite furnace at 1840 or 1855 ◦ C for 16 h. Afterward,
furnace-cooled specimens were finally annealed at 1740 ◦ C for 1 h [23].
The sintering and annealing processes of the AlN ceramics were both
protected by 99.99 vol% N2 at a flowing rate of 50 L/min. Using A, B,
and C three kinds of AlN powders as raw materials, the AlN ceramic
substrates sintered at 1840 ◦ C were named NA1, NB1, and NC1,
respectively; while the AlN ceramic substrates sintered at 1855 ◦ C were
successively named as NA2, NB2, and NC2.
2.2. Characterization
After AlN green bodies were degreased and two sides of the AlN
ceramic substrates were ground and polished to remove the oxide layers,
then their O (lattice O), N, and C contents were tested, as described in
Refs. [23,25]. After the AlN ceramics were sintered and annealed, their
original surfaces were analyzed using an X′ Pert PRO MPD-type X-ray
diffractometer to determine the GB phases of AlN ceramics, following
the X-ray diffraction (XRD) parameters in Ref. [23]. Given the XRD
analysis results, the amount of each GB phase was determined via the
RIR method indicated in Ref. [23]. After thin Au coatings were deposited
onto AlN ceramics using a Model 682-type ion sputtering coating in­
strument, surface and cross-sectional back-scatter electron (BSE) images
of the AlN ceramics were examined using a Gemini 500-type field
emission scanning electron microscopy (SEM). Volume fractions of the
GB phases (VGB) in the AlN ceramics were calculated using the
Image-Pro Plus software, and the AlN grain sizes (d) were determined
following the linear intercept method, as shown in Refs. [23, 26].
After AlN ceramics were ground and polished, the density (ρ) of the
AlN ceramics was measured using the Archimedes method, and the
theoretical density (ρth) was calculated in terms of the rule of mixture, as
densities of the relevant phases of AlN, YAM and Y2O3 were known as
3.26, 4.44, and 5.01 g/cm3 [27,28], respectively. Thus, the relative
density (ρ/ρth) of the AlN ceramics was obtained. Measurements of TC
and bending strength (σ) of the AlN ceramics were also described in
Ref. [23] in detail. Based on the bending strength test, σ and Young’s
modulus, E, of the AlN ceramics were calculated as followed [29]:
σ=
3FL
2bh2
(1)
E=
kL3
4bh3
(2)
where F is the load at failure, and L, b and h are the span (30 mm), width
(4 mm) and thickness (2 mm) of the specimens, respectively. And, k is
the slope of the load-deflection curves (Fig. 6) in the elastic deformation
stage.
Hardness of the AlN ceramics was measured via the Vickers inden­
tation method in a Wilson Model VH-3100 type Vickers hardness tester
using a load of 5 kgf and a dwell time of 10 s. Fracture toughness, KIC, of
the AlN ceramics was determined using the Vickers indentation tech­
nique, and the following equation was employed [29,30]:
(
Items
A
B
C
O/wt%
N/wt%
C/ppm
Fe/ppm
Si/ppm
Ca/ppm
Specific surface areas/(m2/g)
Average particle size (d50)/(μm)
0.87
33.59
350
15
22
216
3.62
1.09
0.76
33.60
287
20
26
236
3.56
1.12
0.64
33.62
269
18
30
227
3.21
1.24
KIC = χ
)1/2 (
)
E
F1
3/2
Hv
a
(3)
where F1 is the applied load (49 N), Hv is the Vickers hardness, a is the
crack propagation length measured from the center of indentation, and χ
is an empirically determined “calibration” constant taken to be 0.016.
Six indentations of each specimen were measured to obtain average Hv
and a values. Noted that this method might have any drawbacks,
because it was susceptible to the specimen surface quality [31].
29633
X. Wei et al.
Ceramics International 50 (2024) 29632–29641
However, the relatively accurate KIC values in this study could be
employed to identify the effects of the GB phase distributions on the
mechanical characteristics of the AlN ceramics. SEM was employed to
observe the indention morphologies in the secondary electron (SE)
model and the crack propagation paths in the BSE model, respectively.
For the R-curve test specimen (40 mm × 4 mm × 2 mm), a single
indentation with different loads of 2, 5, and 10 kgf, respectively, was
applied on the center of the specimen surface. The bending strength of
the indented specimens was measured in the method mentioned above.
Accordingly, the R-curves of the AlN ceramics were plotted, and more
detailed information was available in Section 3.5. For each TC or me­
chanical property test, 3–6 specimens were taken to acquire the average
value.
3. Results and discussion
3.1. Chemical and phase compositions
After the AlN green bodies were degreased, the O contents of the AlN
green bodies corresponded with the O impurity contents of the AlN
powders (Table 2). Free carbon remained in the AlN green bodies was
amorphous and adhered to the AlN particles [32]. About 0.5 wt% of free
carbon in the AlN green bodies effectively removed O impurity, thereby
improving the TC and mechanical properties of the AlN ceramics
[33–35].
Compared with the AlN green bodies, both the O and C contents of
the AlN ceramics were significantly reduced. As the sintering tempera­
ture rose, the O and N contents of the ceramics diminished and
enhanced, respectively. The O content in the 1840 ◦ C sintered AlN ce­
ramics was in a sequence: NC1 > NB1 > NA1, whereas the O content in
the 1855 ◦ C sintered AlN ceramics followed an order: NC2 > NA2 >
NB2, indicating that the AlN ceramic corresponding to the AlN green
body with the lowest O content reversely had the highest O content. The
result is because: (1) The higher the O content of AlN green bodies is, the
more the oxide melt amount of the AlN sintered bodies is. (2) The
migration capability of the oxide melt increased with rising the sintering
temperature. As shown in Fig. 1a–c and e, the oxide melt migrated to­
ward the surfaces of the NB1 and NC1 specimens was smaller than that
migrated toward the NA1 specimen surface during sintering at 1840 ◦ C.
Therefore, the amount of oxide melt remained in the NB1 and NC1
specimens was higher, thus increasing the O content in them. The oxide
melt of the 1855 ◦ C sintered AlN ceramics migrated to the surface of the
NB2 specimen increased, resulting in the O content in the NB2 specimen
decreased (Fig. 1d–Table 2). Meanwhile, the migration of the oxide melt
in the NC2 specimen was relatively lower than that in the NA2 and NB2
specimens, and the NC2 specimen also had higher amount of lattice O
impurity (Fig. 1f–Table 2).
As shown in Fig. 1, the surficial oxide layer was formed through
migration and overflow of the oxide melt from the AlN ceramics during
the sintering process, which had the same compositions as the GB phase
within the AlN ceramic substrates. As the sintering temperature rose, the
migration of the oxide melt toward the ceramic surface was accelerated
[36], leading to thickening of the surficial oxide layer (Fig. 1). As a
result, the AlN diffraction peaks became weak (Fig. 2). The GB phases of
the six kinds of AlN ceramics, namely NA1, NB, NC1 and NA2, NB2,
NC2, were composed of YAM and Y2O3, with YAM being the dominant
one (Table 3). As depicted in Refs. [37,38], the removal of lattice O
promoted the formation of YAM in the GB phase of the AlN ceramic. As
the sintering temperature rose, the Y2O3 content in the GB phases of the
NA1-2/NB1-2 specimens increased/decreased, respectively, while that
remained stable in the GB phases of the NC1-2 specimens (Table 3). It
resulted from a confliction between the exsolution of lattice O to form
YAM and the reduction reaction of YAM with the residual C atoms to
form Y2O3 [12], these two processes were accelerated with rising the
sintering temperature.
3.2. GB phase distributions
During liquid-phase sintering, the oxide melt migrated toward the
AlN ceramic surfaces driven by the capillary force [36]. As depicted in
Fig. 1, the migration extent of oxide melt was positively correlated with
the melt content in the AlN ceramics and the sintering temperature.
Moreover, as the sintering temperature increased, more lattice O
exsolved to increase the melt content, and the melt viscosity decreased.
As a result, more oxide melt overflowed, and the thickness of the sur­
ficial oxide layer increased [36]. However, excessive migration of the
oxide melt reduced the remained melt content in the AlN ceramics, e.g.,
NA2, which was extremely low to fulfill the sintering densification of the
AlN ceramics. Therefore, the porosities of the ceramics increased
(Table 5), which negatively affected the TC and mechanical properties of
the AlN ceramics.
As the sintering temperature rose, the AlN grains in the AlN ceramics
grew normally, with a straight GB and a polyhedral shape, however the
GB phase distributions were relatively different with a varied dihedral
angle (θ) of the GB phase between two AlN grains (Fig. 3). The GB phases
in the NA1 specimen were mainly semi-continuously distributed (θ =
0◦ ), besides a small amount of the GB phase existed at the triple AlN GB
junctions (θ = 33◦ ) (Fig. 3a). In the NA2 specimen, the GB phases were
continuously distributed (θ = 0◦ ) (Fig. 3b), indicating that as the sin­
tering temperature rose, wettability of the oxide melt on the AlN grains
increased, thus enlarging the GB phase/AlN interfaces and then reducing
the AlN GB areas [9,39,40]. The GB phases in the NB1 specimen was
overwhelmingly distributed as isolated islands (Fig. 3c). Because the
isolated island GB phases had a high content, a large size and dihedral
angle (θ = 93◦ or 110◦ ) (Fig. 3c–Table 4), they were named large iso­
lated island particles. In contrast, the GB phase content of the NB2
specimen was only 2.36 % (Table 4), the GB phase particles had a
smaller size, and most of them huddled in the triple AlN GB junctions (θ
= 69◦ ), resulting in the increase of the AlN GB area of the NB2 specimen
(Fig. 3d). In the NC1-2 specimens, the GB phases had high contents and
sizes, which were densely distributed among the AlN grains as large
isolated island particles (θ = 120◦ or 115◦ ) (Fig. 3e and f, Table 4). With
decrease of the large isolated island-like GB phases, and increase of the
fine GB phases at the triple AlN GB junctions, the θ values were
decreased. Some GB phase particles were interconnected to segment the
AlN grains. In the AlN ceramics containing semi-continuous/continuous
GB phases (NA1 and NA2), the AlN grain was contacted with the GB
phase through a 1–3 nm thickness amorphous layer, according to the
TEM results in Ref. [23]. The weak amorphous layer interface was
believed to provide a preferential path for crack propagation. The high
thermal mismatch between the GB phases such as YAM and Y2O3 and the
AlN grains due to their apparent CTE differences [15,18] induced re­
sidual thermal stress at the GB phase/AlN interface, further affecting
fracture strength and crack propagation mode of the AlN ceramics [4,5].
Table 2
Elemental compositions of the AlN green bodies and ceramics (wt%).
Elements
O (Lattice O)
N
C
Green bodies
Ceramics
A
B
C
NA1
NA2
NB1
NB2
NC1
NC2
1.90
32.36
0.53
1.82
32.41
0.53
1.73
32.48
0.52
0.86(0.06)
31.68
–
0.83(0.06)
31.79
–
0.90(0.08)
31.63
–
0.77(0.05)
31.88
–
0.94(0.08)
31.59
–
0.85(0.08)
31.75
–
29634
X. Wei et al.
Ceramics International 50 (2024) 29632–29641
Fig. 1. Cross-sectional BSE-SEM images showing the oxide layers on the AlN ceramic surfaces and the GB phase distributions in the AlN ceramics (a) NA1; (b) NA2;
(c) NB1; (d) NB2; (e) NC1; (f) NC2.
Table 3
Phase compositions and contents (wt%) of the GB phases in the AlN ceramics.
Fig. 2. XRD patterns of the AlN ceramics of different oxygen contents sintered
at various temperatures.
Specimen codes
YAM
Y2O3
NA1
NA2
NB1
NB2
NC1
NC2
72.65
70.72
75.40
82.79
78.65
78.15
27.35
29.28
24.60
17.21
21.35
21.85
In the AlN ceramics, the GB phases with the large isolated island parti­
cles or the fine ones at the triple AlN GB junctions (NB1-2 and NC1-2)
evoked a compressive stress at the AlN GBs adjacent to the GB phase
particles. The compressive stress inhibited crack propagation along the
AlN GBs [15,22], and the bonding of the AlN GBs was strengthened, and
even larger than the cleavage fracture strength of the AlN grains,
thereby some AlN grains preferred to the transgranular fracture mode. In
contrast, the tensile stress existed at the continuous/semi-continuous GB
phase/AlN interface (NA2) and thus the crack propagated preferentially
along the interface in the intergranular fracture mechanism [15,19].
In summary, in the AlN ceramics of high O impurity contents, i.e.,
NA1-2, more oxide melt was formed during sintering, which constructed
a connected network, facilitating melt migration toward the AlN
ceramic surfaces. After that, the oxide melt network entirely/partly
29635
Ceramics International 50 (2024) 29632–29641
X. Wei et al.
Fig. 3. Cross-sectional BSE-SEM images showing the GB phase distributions in the AlN ceramics (a) NA1; (b) NA2; (c) NB1; (d) NB2; (e) NC1; (f) NC2.
Table 4
Microstructural data of the AlN ceramics.
Specimen codes
AlN grain size (d)/(μm)
Content of the GB phase (VGB)/(vol%)
NA1
NA2
NB1
NB2
NC1
NC2
7.05
7.21
6.36
6.51
6.07
6.45
1.78
1.73
3.15
2.36
4.82
3.37
3.3. Bending strengths
Table 5
Thermal and mechanical properties of the AlN ceramics.
Specimen
codes
ρ/(g/
ρth/(g/
cm3)
Relative
densities/(%)
TC/(W/
(m⋅K))
σ/(MPa)
NA1
3.25 ±
0.01
3.24 ±
0.01
3.27 ±
0.01
3.25 ±
0.01
3.29 ±
0.01
3.28 ±
0.01
3.28
99.08
3.28
98.78
3.30
99.09
3.28
99.09
3.33
98.80
3.31
99.09
220.45 ±
2.88
210.18 ±
2.67
207.83 ±
2.03
230.09 ±
1.15
198.98 ±
1.56
207.53 ±
2.25
400.52 ±
5.24
332.21 ±
5.76
458.70 ±
3.61
432.85 ±
6.04
428.36 ±
3.91
421.64 ±
5.84
NA2
NB1
NB2
NC1
NC2
cm3)
remained, and transferred into the continuous/semi-continuous GB
phases in the AlN ceramics. However, the connected networks in the AlN
ceramics with low O contents, i.e., NB1-2 and NC1-2, were only formed
at higher sintering temperature of 1855 ◦ C. More oxide melt remained
and transferred into the GB phases in the AlN ceramics as large isolatedisland particles and/or fine particles at the triple AlN GB junctions
(Fig. 3).
Six kinds of AlN ceramics developed in this work all had high TCs
about 200 W/(m⋅K) and above, however their bending strengths were
variable (Table 5). The relatively low deviations in the density, TC and
bending strength tests indicated a high microstructural stability of the
AlN ceramics. As shown in Fig. 1, the oxide melt migrated from the NA12 specimens was the largest in amount, therefore the remained oxide
melt in the specimens was relatively low in amount, existing as the
continuous/semi-continuous GB phase in the AlN ceramics. As a result,
the specimens had increasing porosity and decreasing relative density,
thus decreasing bending strength (Table 5). The surficial oxide layer of
the NB1 specimen was thin, and more GB phase remained, acting as
large isolated island particles in the specimen. It leaded to the highest
bending strength (458.7 MPa) of the AlN ceramic. The NB2 specimen
had the lowest lattice O and rather low GB phase content (Tables 2 and
4). It had the highest relative density (Table 5), and more GB phases
were fine at the triple AlN GB junctions to strengthen the AlN GBs. As a
29636
X. Wei et al.
Ceramics International 50 (2024) 29632–29641
result, the NB2 specimen had the second highest bending strength
(432.85 MPa) and the highest TC (230.09 W/(m⋅K)), because the seg­
mentation effect of the GB phases was greatly diminished, and the GB
strengthening effect was enhanced. The NC1-2 specimens had a large
amount of GB phase and the largest GB phase size, as a result, they had
medium-level relative density and bending strength.
In this study, the AlN ceramics fabricated by pressureless sintering at
1855 ◦ C for 16 h and annealing at 1740 ◦ C for 1 h exhibited remarkable
comprehensive performance. The comprehensive performance sur­
passed all of the previously reported AlN ceramics prepared via similar
pressureless sintering and annealing processes (Table 6).
3.4. Fracture toughness and fracture mechanism
In order to evaluate effect of the GB phase distribution on the frac­
ture toughness and R-curve characteristics of the high-TC AlN ceramics,
three kinds of AlN ceramic specimens, i.e. NA2, NB2, and NC2 sintered
at 1855 ◦ C, were subsequently employed. The load-deflection (F-Δl)
curves of the NA2, NB2, and NC2 specimens during three-point bending
were shown in Fig. 4. Under the applied loads, the NB2 specimen had the
highest load-bearing capacity, following by the NC2 specimen, and the
NA2 specimen was the last. The slopes (k) of the F-Δl curves in the elastic
deformation stage were kNB2 = 1524, kNC2 = 1499, and kNA2 = 1458 for
the three specimens, respectively. After assigning these k values into Eq.
(2), the E values of the NA2, NB2, and NC2 specimens were obtained.
Thereafter, by testing the Vickers hardness (Hv, Table 7), the fracture
toughness (KIC) of the AlN ceramics were calculated in Eq. (3), as listed
in Table 7.
As shown in Table 7, the testing deviations of these mechanical
property indexes were all in low levels. The Hv and E values of the NB2
and NC2 specimens were significantly higher than those of the NA2
specimen, because of higher relative densities of them (Table 5).
Because the AlN grain sizes of three kinds of AlN ceramics were nearly
equivalent (Table 4), the AlN grain size might not be the key influencing
factor to the strength and toughness of the AlN ceramics [41]. For the
NB2 and NC2 specimens, the isolated island-like GB phase distribution
could enhance the AlN GBs, and thus inhibit crack propagation,
compared with the NA2 specimen of the continuous/semi-continuous
GB phase distribution. As a result, the a values of the NB2 and NC2
specimens were reduced, but the strength, hardness, elastic modulus,
and fracture toughness of them were increased (Table 7).
The surface indentation and crack propagation of the NA2, NB2, and
NC2 specimens under a load of 5 kgf were illustrated in Fig. 5. The in­
dentations of all specimens exhibited a regular diamond shape, and
surface cracks of varying lengths initiated at the four corner positions
(Fig. 5a–c, e). The cracks preferentially propagated along the AlN GBs
and the GB phase/AlN grain interfaces in the NA2 specimen, indicating
that under the applied load, the intergranular fracture of the NA2
specimen overwhelmingly occurred. Meanwhile, the transgranular
fracture of a small number of AlN grains and GB phases also took place,
as indicated in the red arrows in Fig. 5b. Similarly, surface cracks mainly
extended along the AlN GBs and the GB phase/AlN grain interfaces,
partly through the AlN grains and GB phases of the NB2 and NC2
Fig. 4. Load-deflection relationship curves of the AlN ceramic specimens.
Table 7
Mechanical properties of Hv, E and KIC of the AlN ceramics.
Specimen
codes
Hv/(GPa)
E/(GPa)
a/(mm)
KIC/(MPa⋅m1/
2
)
NA2
7.78 ±
0.14
8.85 ±
0.10
8.77 ±
0.13
307.60 ±
4.05
321.42 ±
3.17
316.23 ±
3.72
0.133 ±
0.003
0.117 ±
0.002
0.119 ±
0.002
3.21 ± 0.18
NB2
NC2
3.73 ± 0.16
3.64 ± 0.15
specimens, as indicated in the red arrows in Fig. 5d and f. However, the
NB2 and NC2 specimens have lower a values (Table 7), and higher
fraction of transgranular fracture (̂f ) of the AlN grains and GB phases
(Table 8) than the NA2 specimen. Additionally, crack branching easily
took place at the AlN GBs adjacent to the isolated island-like GB phases,
as indicated in the green arrows in Fig. 5d–f. The strength and toughness
of the AlN ceramics were therefore increased through strengthening the
AlN GBs to increase the crack propagation resistance. However,
although the NA2 specimen had a non-ideal GB phase structure, i.e., the
continuous/semi-continuous GB phase, the toughness of the specimen
was not too low, due to more tortuous paths of the intergranular fracture
than those of the transgranular fracture [43–45].
As mentioned above, the proportion of the two fracture mechanisms,
i.e., ̂f , was a function of various factors. As reported previously, the
phase-field model and etc were used to study the effects residual stress
on fracture toughness, and further to reveal the fracture characteristics
of dual-phase ceramics [46,47]. However, the model of the difference
between the released energy of the intergranular crack propagation and
that of the transgranular crack propagation and the theory concerning
Table 6
Comparison of the properties of several AlN ceramics prepared by pressureless sintering.
Sintering additives
Sintering parameters
Annealing parameters
TC/(W/(m⋅K))
σ/(MPa)
Refs.
4.9 wt% Y2O3
8.0 wt% Y2O3
1 wt% CaZrO3+1 wt% Y2O3
3 wt% CaZrO3+3 wt% Y2O3
4 wt% CeO2+1 wt% Y2O3
4 wt% CeO2+1 wt% Y2O3
1 wt% MgO–CaO–Al2O3–SiO2+3 wt% Y2O3+1 wt% ZrO2
5 wt% Sm2O3
5.2 wt% Y2O3
1850 C, 2 h
1855 ◦ C, 10 h
1600 ◦ C, 3 h
1600 ◦ C, 3 h
1600 ◦ C, 12 h
1800 ◦ C, 12 h
1600 ◦ C, 1 h
1850 ◦ C, 2 h
1900 ◦ C, 100 h
–
–
1400 C, 2 h
1400 ◦ C, 2 h
–
–
–
–
–
180
205
132
156
136
180
109
176
272
495
295
592
560
433
311
608
455
–
[19]
[17]
[21]
[21]
[41]
[41]
[22]
[35]
[38,42]
◦
◦
29637
Ceramics International 50 (2024) 29632–29641
X. Wei et al.
Fig. 5. (a, c, e) SE− SEM images showing the indentations on the NA2, NB2 and NC2 specimens, and (b, d, f) BSE-SEM images showing crack propagation states in
Areas 1–3 in Figs. a, c and f, respectively.
generally acknowledged that certain a path of the lowest released energy
acted as the most preferential crack propagation path. Therefore, the
crack path could be confirmed via comparing the released energy of the
intergranular crack propagation and that of the transgranular crack
propagation. When a crack propagated in the selected region of the
intergranular fracture with a length of yc, the ̂f and the critical energy
release rate (GIC) were expressed as functions of the AlN grain size (d),
grain
energy release rate of AlN grain (GIC
̂f = 1-2yc
d
(4)
(
)
{
2yc
p 2 q } 2yc
GIC = Ggrain
y + yc
1+ GGB
IC
IC 1 +
6d c 2d
d
d
(5)
yc =
⎧
√̅̅̅̅̅̅̅̅̅̅̅̅̅̅̅̅̅̅̅̅̅̅̅̅̅̅̅̅̅̅̅̅̅̅̅̅̅̅̅̅̅
(
)
√
⎪
grain
⎪
√
⎪
⎪
√q2 + 2 GIC -1 pd
⎪
-q
+
⎪
⎪
GGB
⎨
IC
grain
, and GGB
IC values of the AlN specimens.
Specimen codes
̂f /(%)
grain
GIC /(J/m2)
2
GGB
IC /(J/m )
NA2
NB2
NC2
4.36
28.07
25.19
60.05
60.82
60.34
7.50
10.55
10.09
the influence of the crack path on the fracture toughness of poly­
crystalline ceramics [35,48,49] were introduced in the fracture char­
acteristic research on the AlN ceramics in the current work. It was
p=
8
pʹ
2a
(d ≥ d∗ )
(6)
d
(0 < d < d∗ )
2
(
d∗ =
Calculated ̂f , GIC
p
⎪
⎪
⎪
⎪
⎪
⎪
⎪
⎩
Fig. 6. Linear fitting curves of lgσ m of the AlN indentation specimens varied
with lgF1.
Table 8
) and GB (GGB
IC ) [35,48,49]:
grain
GIC
GGB
IC
)
-1 -4q
p
(7)
(8)
where p’ and q are constants, and equal to 9.5 × 102 and 8.5 [48],
respectively. d* refers to the critical grain size of the transgranular
fracture. According to Ref. [35], the ̂f of the AlN ceramics was obtained
through analyzing the fracture modes of more than 200 grains in the
SEM images, as listed in Table 8. Therefore, it was concluded that the ̂f
of the NB2 specimen was the maximal, that of the NA2 specimen was the
29638
X. Wei et al.
Ceramics International 50 (2024) 29632–29641
minimal, and that of the NC2 specimen fell in between, because of the
different GB phase distributions of these three AlN ceramics.
According to Irwin’s equation, GIC could be calculated as [48–50]:
(
)
K2IC 1-v2AlN
GIC =
(9)
E
where vAlN is Poisson ratio of the AlN ceramics (0.25). The values of KIC,
E, a, d and ̂f in Tables 7 and 8 were substituted into Eqs. (4)–(9)
grain
respectively, and the GIC and GGB
IC of the three AlN ceramics were
calculated, as listed in Table 8.
Because the GB phase contents in the three AlN specimens were
extremely low (Table 4), and the transgranular fracture areas of the GB
phases were small (Figs. 3 and 5), the transgranular fracture of the GB
phases was then ignored, and hence the transgranular fracture of the AlN
grain
ceramics was approximately equal to that of the AlN grains. The GIC
values of the three AlN ceramics were close to each other. As indicated in
Ref. [35], the lattice oxygen in the AlN grains tended to form vacancies
and stacking faults, resulting in reduction of the fracture toughness of
the AlN ceramics. Herein, the lattice oxygen contents of the three
high-TC AlN ceramics were in a very low level (Table 2), so the influence
of the lattice oxygen on the fracture toughness of the AlN grains was
much limited. As far as the GGB
IC of the three AlN ceramics was concerned,
the NB2 specimen (10.55 J/m2) was slightly higher than the NC2
specimen (10.09 J/m2), but they were both significantly higher than the
NA2 specimen (7.50 J/m2). So, the ̂f and GGB could act as the indicators
IC
of the strength, toughness and fracture mechanism of the three AlN
ceramics. In the NA2 specimen, the continuous/semicontinuous GB
phase segmented the AlN grains, resulting in the low GB phases/AlN
interface bonding strength, the low ̂f and GGB , and thus the low strength
IC
and toughness of the AlN ceramic. In contrast, the isolated island-like GB
phase particles, no matter the particle size, had less segmentary effect on
the AlN grains, and induced a compressive stress at the AlN GBs, in the
NB2 and NC2 specimens. As a result, the crack propagation resistance
was increased, and further the ̂f , GGB , and strength-toughness of the AlN
IC
ceramics were enhanced.
3.5. R-curve characteristics
where kR and m are material constants. In general, the relationship be­
tween the σ m and the indentation load, F1, obeyed the following equa­
tion [52]:
σ m = AF1 -B
(11)
Taking the σm and F1 values in Table 9 into Eq. (11), a linear fitting
curve of lgσ m ~ lgF1 for each AlN indentation specimen was established,
as shown in Fig. 6. Next, the A and B values in Eq. (11) were determined,
corresponding to the slope and its intercept on the ordinate of the curve,
respectively. Finally, the kR and m values in Eq. (10) could be calculated
via the following equations [52]:
m = (1-3B)/(2 + 2B)
(14)
kR = YA(Bγ)-B (1 + B)(1+B)
(15)
γ = F1
/(
a2/(1+B)
)
(16)
where Y is a dimensionless configuration coefficient that is dependent
on the boundaries of the specimen (1.174). Therefore, the R-curves of
the three AlN ceramic specimens were plotted, as shown in Fig. 7.
As shown in Fig. 7, it was evident that the R-curve effect [52,53] of
the AlN ceramic specimens was obvious. The slope of the R-curve was
large in the initial stages of crack propagation, leading to a rapid in­
crease of KR, and it was decreased, when the crack continued to extend.
Additionally, the R-curve effect of the three AlN ceramics was different
due to their different microstructures. Hypothesizing the a value
increased from 0.10 mm (just below the minimal a value of all specimens
in this work (Table 7)) to 2.00 mm in the AlN ceramics, based on Refs.
[35,52], the predicted maximal KR value of the R-curves, KR,max, was
different for the different specimens. The KR,max of the NA2 specimen
was as low as 4.66 MPa m1/2, however that of the NB2 specimen was the
highest (5.13 MPa m1/2). The KR,max of the NC2 specimen was 4.96 MPa
m1/2, more close to that of the NB2 specimen, but slightly lower. It was
concluded that the sequence of the crack propagation resistance was
NB2>NC2>NA2 for the three AlN ceramics, attributing to that the GB
phases in the NB2, NC2 ceramics were composed of the large isolated
island particles or the fine ones at the triple AlN GB junctions, which
could effectively enhance the AlN GBs. Such a reinforcing effect further
inhibited crack propagation, and thus improved the ̂f , GGB and the
IC
After forming indentation at the central positions on surfaces of the
NA2, NB2, and NC2 specimens by loads of 2, 5, and 10 kgf, three-point
bending strength (σ m) of the specimens was tested, as setting the
indentation surfaces downward, and the results were listed in Table 9.
As the applied load increased, the surface crack length of the indentation
specimen increased, leading to a significant decrease of σm [51]. Under a
certain load, the sequence of σ m was NB2>NC2>NA2 for the AlN ce­
ramics, which was consistent with the σ order of three ceramics without
indentation specimens (Table 5).
In the fracture process of the AlN indentation specimens, the R-curve
denoted to the relationship between the critical stress intensity factor,
KR, and a, which was described by Eq. (10) provided by Krause et al.
[52]:
KR = kR am
fracture toughness of the ceramics.
In summary, the high-quality AlN ceramic substrates could be
manufactured in terms of choosing low O content AlN powder as the raw
material, and optimizing the technical parameters of presureless sin­
tering and subsequent heat treatment. During presureless sintering and
subsequent heat treatment, purification of the AlN lattice, migration and
(10)
Table 9
Bending strength (MPa) of the indentation AlN ceramic specimens under
different indentation loads.
Specimen codes
NA2
NB2
NC2
Indentation load/(kgf)
2
5
10
165.21 ± 2.61
196.03 ± 2.56
188.28 ± 3.00
140.45 ± 2.48
160.51 ± 2.78
153.26 ± 2.52
113.17 ± 2.95
133.40 ± 2.23
128.43 ± 1.79
Fig. 7. R-curves of the AlN specimens.
29639
Ceramics International 50 (2024) 29632–29641
X. Wei et al.
overflow of the oxide melt to the AlN ceramic surface promoting, and
crystallization transformation of the GB phases were fulfilled as much as
possible. More importantly, the GB phases were distributed in the AlN
ceramics in the isolated island-like state, optimally situated in the triple
AlN GB junctions, instead of the continuous/semi-continuous state. In
this situation, the AlN GBs were strengthen to increase the crack prop­
agation resistance, the ̂f and GGB of the AlN ceramics were significantly
IC
improved. The AlN ceramics have great comprehensive performance of
high σ , KIC, R-curve characteristic, and TC, and then a high reliability to
withstand thermal and mechanical shock.
4. Conclusions
1. The high-TC AlN ceramics of different GB phase distributions were
fabricated using the AlN powders with different O impurity contents
as raw material, and pressureless sintering at various temperature.
The GB phases mainly consisted of YAM and Y2O3, and approxi­
mately exhibited three different states of continuous/semicontinuous phase, large isolated island-like particles, and the fine
particles at the triple AlN GB junctions.
2. With decrease of the large isolated island-like GB phases, and in­
crease of the fine GB phases at the triple AlN GB junctions, the
dihedral angle of the GB phases decreased, and the compressive
stress at the AlN GBs increased. It was beneficial to enhancement of
bending strength and fracture toughness of the AlN ceramics.
Comparatively, the semi-continuous/continuous GB phase segre­
gated the AlN grains, and induced the GB phase/AlN interface tensile
stress, resulting in the lowest bending strength and fracture tough­
ness of the AlN ceramics.
3. The high-TC AlN ceramics principally followed the intergranular
fracture mode, but with different transgranular fracture fractions.
The AlN ceramics with the continuous/semicontinuous GB phases
had the lower fraction of transgranular fracture, while those with the
isolated island-like GB phases possessed higher fraction of trans­
granular fracture. Moreover, the isolated island-like GB phases could
strengthen the AlN GBs, and also induce the crack deflection and
branching, as a result, the crack propagation in the ceramics was
inhibited.
4. The R-curve effect of the high-TC AlN ceramics was obvious. The
continuous GB phase/AlN interface exhibited the toughness and GB
energy release rate, and thus lowered the crack propagation resis­
tance and reliability of the AlN ceramics. In contrast, the AlN ce­
ramics with the isolated island-like GB phase particles, especially the
fine particles at the triple AlN GB junctions, owned higher interface
toughness and GB energy release rate, and hence higher crack
propagation resistance and reliability.
CRediT authorship contribution statement
Xin Wei: Writing – original draft, Methodology, Investigation, Data
curation. Hao Zhang: Resources, Data curation. Junjie Dang: Valida­
tion, Investigation. Haixian Xu: Resources, Investigation. Jun Guo:
Validation, Investigation. Jingwei Li: Visualization, Investigation. Song
Cui: Supervision, Project administration. Wenming Tang: Writing –
review & editing, Supervision, Funding acquisition.
Declaration of competing interests
The authors declare that they have no known competing financial
interests or personal relationships that could have appeared to influence
the work reported in this paper.
Acknowledgements
This work was financially supported by Projects of Scientific and
Technological Research, Anhui Province,
202004a05020022, 202003a05020006).
China
(Grants
Nos.
References
[1] T. Kusunose, T. Sekino, K. Niihara, Production of a grain boundary phase as
conducting pathway in insulating AlN ceramics, Acta Mater. 55 (18) (2007)
6170–6175, https://doi.org/10.1016/j.actamat.2007.07.025.
[2] H. Jiang, X.H. Wang, W. Lei, G.F. Fan, W.Z. Lu, Effects of two-step sintering on
thermal and mechanical properties of aluminum nitride ceramics by impedance
spectroscopy analysis, J. Eur. Ceram. Soc. 39 (2019) 249–254, https://doi.org/
10.1016/j.jeurceramsoc.2018.09.026.
[3] P. Kaya, Y.E. Suyolcu, P.A.V. Aken, S. Turan, G. Gregori, J. Maier, Grain boundary
blocking effects in Sm/Yb-doped AlN ceramics, J. Eur. Ceram. Soc. 41 (2021)
4870–4875, https://doi.org/10.1016/j.jeurceramsoc.2021.03.033.
[4] H.M. Lee, D.K. Kim, High-strength AlN ceramics by low-temperature sintering with
CaZrO3–Y2O3 co-additives, J. Eur. Ceram. Soc. 34 (15) (2014) 3627–3633, https://
doi.org/10.1016/j.jeurceramsoc.2014.05.008.
[5] A.T. Wieg, Y. Kodera, Z. Wang, C. Dames, J.E. Garay, Thermomechanical
properties of rare-earth-doped AlN for laser gain media: the role of grain
boundaries and grain size, Acta Mater. 86 (2015) 148–156, https://doi.org/
10.1016/j.actamat.2014.11.045.
[6] J.D. Clayton, Penetration resistance of armor ceramics: dimensional analysis and
property correlations, Int. J. Impact Eng. 85 (2015) 124–131, https://doi.org/
10.1016/j.ijimpeng.2015.06.025.
[7] G.R. Johnson, T.J. Holmquist, S.R. Beissel, Response of aluminum nitride
(including a phase change) to large strains, high strain rates, and high pressures,
J. Appl. Phys. 94 (3) (2003) 1639–1646, https://doi.org/10.1063/1.1589177.
[8] R. Lee, Development of high thermal conductivity aluminum nitride ceramic,
J. Am. Ceram. Soc. 74 (9) (1991) 2242–2249, https://doi.org/10.1111/j.11512916.1991.tb08291.x.
[9] J. Zhan, Y. Cao, H. Zhang, J. Guo, J.H. Zhang, C.L. Geng, C.D. Shi, S. Cui, W.
M. Tang, Low-temperature sintering of AlN ceramics by sm2O3-Y2O3-CaO sintering
additives formed via decomposition of nitrate solutions, J. Mater. Eng. Perform. 26
(1) (2017) 453–459, https://doi.org/10.1007/s11665-016-2453-1.
[10] G.L. Nie, P.F. Sheng, Y.H. Li, F. Zuo, Y.W. Bao, S.H. Wu, Enhanced mechanical and
thermal properties of AlN ceramics via a chemical precipitation process, Int. J.
Appl. Ceram. Technol. 18 (4) (2021) 1255–1268, https://doi.org/10.1111/
ijac.13742.
[11] T. Barrett Jackson, AnilV. Virkar, High-thermal-conductivity aluminum nitride
ceramics: the effect of thermodynamic, kinetic, and microstructural factors, J. Am.
Ceram. Soc. 80 (6) (1997) 1421–1435, https://doi.org/10.1111/j.11512916.1997.tb03000.x.
[12] K. Watari, H.J. Hwang, M. Toriyama, S. Kanzaki, Effective sintering additives for
low-temperature sintering of AlN ceramics, J. Mater. Res. 14 (4) (1999)
1409–1417, https://doi.org/10.1557/JMR.1999.0191.
[13] G. Pezzotti, A. Nakahira, M. Tajika, Effect of extended annealing cycles on the
thermal conductivity of AlN/Y2O3 ceramics, J. Eur. Ceram. Soc. 20 (9) (2000)
1319–1325, https://doi.org/10.1016/S0955-2219(99)00286-1.
[14] S. Kume, M. Yasuoka, N. Omura, K. Watari, Effects of annealing on dielectric loss
and microstructure of aluminum nitride ceramics, J. Am. Ceram. Soc. 88 (11)
(2005) 3229–3231, https://doi.org/10.1111/j.1551-2916.2005.00556.x.
[15] F.M. Xu, Z.J. Zhang, X.L. Shi, Y. Tan, J.M. Yang, Effects of adding yttrium nitrate
on the mechanical properties of hot-pressed AlN ceramics, J. Alloys Compd. 509
(35) (2011) 8688–8691, https://doi.org/10.1016/j.jallcom.2011.05.110.
[16] P.S.D. Baranda, A.K. Knudsen, E. Ruh, Effect of yttria on the thermal conductivity
of aluminum nitride, J. Am. Ceram. Soc. 77 (7) (1994) 1846–1850, https://doi.
org/10.1111/j.1151-2916.1994.tb07060.x.
[17] D. Huang, Z.B. Tian, W. Cui, L.Q. Gao, Z. Liu, X.G. Diao, G.H. Liu, Effects of Y2O3
and yttrium aluminates as sintering additives on the thermal conductivity of AlN
ceramic substrates, Ceram. Int. 44 (16) (2018) 20556–20559, https://doi.org/
10.1016/j.ceramint.2018.07.178.
[18] J.H. Koh, E. Sorge, T.C. Wen, D.K. Shetty, Thermal expansion behaviors of yttrium
tungstates in the WO3–Y2O3 system, Ceram. Int. 39 (7) (2013) 8421–8427, https://
doi.org/10.1016/j.ceramint.2013.04.024.
[19] A. Klimera, F. Raether, J. Ruska, Improving strength by controlling segregation in
liquid phase sintered aluminium nitride ceramics, J. Eur. Ceram. Soc. 27 (2–3)
(2007) 1419–1424, https://doi.org/10.1016/j.jeurceramsoc.2006.04.098.
[20] T.S. Suzuki, T. Uchikoshi, Y. Sakka, Effect of sintering additive on crystallographic
orientation in AlN prepared by slip casting in a strong magnetic field, J. Eur.
Ceram. Soc. 29 (12) (2009) 2627–2633, https://doi.org/10.1016/j.
jeurceramsoc.2009.03.015.
[21] H.M. Lee, D.K. Kim, High-strength AlN ceramics by low-temperature sintering with
CaZrO3–Y2O3 co-additives, J. Eur. Ceram. Soc. 34 (15) (2014) 3627–3633, https://
doi.org/10.1016/j.jeurceramsoc.2014.05.008.
[22] S.H. Baek, H. Jeong, S.S. Ryu, AlN with high strength and high thermal
conductivity based on an MCAS-Y2O3-YSZ multi-additive system, J. Eur. Ceram.
Soc. 42 (3) (2022) 898–904, https://doi.org/10.1016/j.jeurceramsoc.2021.11.012.
[23] X. Wei, H. Zhang, J.J. Dang, H.X. Xu, R.J. Zheng, J. Guo, S. Cui, J.H. Zhang, W.
M. Tang, Phase and microstructure optimization of grain boundary oxides and its
effect on the thermal conductivity of Y2O3-doped AlN ceramics, J. Eur. Ceram. Soc.
42 (12) (2022) 4855–4865, https://doi.org/10.1016/j.jeurceramsoc.2022.05.042.
[24] X. Wei, H. Zhang, D.Q. Sun, C.G. Tian, J. Guo, S. Cui, W.M. Tang, Studies on the
Al2OC mesophase in synthesized AlN powder and its effects on properties of AlN
29640
X. Wei et al.
ceramic substrates, Ceram. Int. 46 (13) (2020) 21172–21181, https://doi.org/
10.1016/j.ceramint.2020.05.195.
[25] A. Thomas, G. Müller, Determination of the Concentration of oxygen dissolved in
the AlN lattice by hot gas extraction from AlN ceramics, J. Eur. Ceram. Soc. 8 (1)
(1991) 11–19, https://doi.org/10.1016/0955-2219(91)90087-G.
[26] G.F. Xu, Tayo Olorunyolemi, OttoC. Wilson, IsabelK. Lloyd, Yuval Carmel,
Microwave sintering of high-density, high thermal conductivity AlN, J. Mater. Res.
Soc. 17 (11) (2002) 2837–2845, https://doi.org/10.1557/jmr.2002.0412.
[27] Y.C. Zhou, H.M. Xiang, X.P. Lu, Z.H. Feng, Z.P. Li, Theoretical prediction on
mechanical and thermal properties of a promising thermal barrier material:
Y4Al2O9, J. Adv. Ceram. 4 (2) (2015) 83–93, https://doi.org/10.1007/s40145-0150140-6.
[28] Matweb, Yttrium oxide (Y2O3). https://www.matweb.com/search/DataSheet.asp
x?MatGUID=0253f69251e648bb9e4cf684701b44c0, 2023. (Accessed 20
November 2023).
[29] X.J. Zhao, D.L. Chen, H.Q. Ru, N. Zhang, Zirconium nitride nano-particulate
reinforced Alon composites: fabrication, mechanical properties and toughening
mechanisms, J. Eur. Ceram. Soc. 31 (5) (2011) 883–892, https://doi.org/10.1016/
j.jeurceramsoc.2010.11.014.
[30] J. J Kruzic, R.O. Ritchie, Determining the toughness of ceramics from Vickers
indentations using the crack-opening displacements: an experimental study, J. Am.
Ceram. Soc. 86 (8) (2003) 1433–1436, https://doi.org/10.1111/j.11512916.2003.tb03490.x.
[31] G.D. Quinn, Fracture toughness of ceramics by the Vickers indentation crack length
method: a critical review, in: R. Tandon, A. Wereszczak, E. Lara-Curzio (Eds.),
Mechanical Properties and Performance of Engineering Ceramics and Composites
II, Wiley Inc., 2007, pp. 45–62.
[32] H.W. Yan, W.R. Cannon, D.J. Shamfield, Evolution of carbon during burnout and
sintering of tape-cast aluminum nitride, J. Am. Ceram. Soc. 76 (1) (1993) 166–172,
https://doi.org/10.1111/j.1151-2916.1993.tb03702.x.
[33] F. Ueno, A. Horiguchi, Grain boundary phase elimination and microstructure of
aluminum nitride, in: Proc. 1st Eur. Ceram. Soc. Conf., Elsevier Appl. Sci., London,
New York, 1989, pp. 383–387.
[34] K. Watari, M.E. Brito, M. Yasuoka, M.C. Valecillos, S. Kanzaki, Influence of powder
characteristics on sintering process and thermal conductivity of aluminum nitride
ceramics, J. Ceram. Soc. Jpn. 103 (9) (1995) 891–900.
[35] R. Terao, J. Tatami, T. Meguro, K. Komeya, Fracture behavior of AlN ceramics with
rare earth oxides, J. Eur. Ceram. Soc. 22 (7) (2002) 1051–1059, https://doi.org/
10.1016/S0955-2219(01)00422-8.
[36] R. Fu, K. Chen, S. Agathopoulos, M.C. Ferro, D.U. Tulyaganov, J.M.F. Ferreira,
Migration of liquid phase in low temperature sintering of AlN, J. Mater. Sci. 40
(9–10) (2005) 2425–2429, 10.1007%2Fs10853-005-1969-9.
[37] K. Watari, M. Kawamoto, K. Ishizaki, Sintering chemical reactions to increase
thermal conductivity of aluminium nitride, J. Mater. Sci. 26 (17) (1991)
4727–4732, https://doi.org/10.1007/BF00612411.
[38] H. Nakanoa, K. Wataric, K. Urabe, Grain boundary phase in AlN ceramics fired
under reducing N2 atmosphere with carbon, J. Eur. Ceram. Soc. 23 (10) (2003)
1761–1768, https://doi.org/10.1016/S0955-2219(02)00408-9.
[39] Y.D. Yu, A.M. Hundere, R. Høier, R.E. Dunin-Borkowski, M.A. Einarsrud,
Microstructural characterization and microstructural effects on the thermal
Ceramics International 50 (2024) 29632–29641
conductivity of AlN(Y2O3) ceramics, J. Eur. Ceram. Soc. 22 (2) (2002) 247–252,
https://doi.org/10.1016/S0955-2219(01)00252-7.
[40] M. Tajika, H. Matsubara, W. Rafaniello, Effect of grain contiguity on the thermal
diffusivity of aluminum nitride, J. Am. Ceram. Soc. 82 (6) (1999) 1573–1575,
https://doi.org/10.1111/j.1151-2916.1999.tb01958.x.
[41] T. Kusunose, T. Sekino, Improvement in fracture strength in electrically conductive
AlN ceramics with high thermal conductivity, Ceram. Int. 42 (11) (2016)
13183–13189, https://doi.org/10.1016/j.ceramint.2016.05.110.
[42] H. Nakano, K. Watari, H. Hayashi, K. Urabe, Microstructural characterization of
high-thermal-conductivity aluminum nitride ceramic, J. Am. Ceram. Soc. 85 (12)
(2002) 3093–3095, https://doi.org/10.1111/j.1151-2916.2002.tb00587.x.
[43] K.T. Faber, A.G. Evans, Intergranular crack-deflection toughening in silicon
carbide, J. Am. Ceram. Soc. 66 (6) (1983) 94–96, https://doi.org/10.1111/j.11512916.1983.tb10084.x.
[44] J.D. Clayton, W.S. Rubink, V. Ageh, D. Choudhuri, R.R. Chen, J. Du, T.W. Scharf,
Deformation and failure mechanics of boron carbide-titanium diboride composites
at multiple scales, JOM 71 (2019) 2567–2575, https://doi.org/10.1007/s11837019-03548-y.
[45] W.S. Rubink, V. Ageh, H. Lide, N.A. Ley, M.L. Young, D.T. Casem, E.J. Faierson, T.
W. Scharf, Spark plasma sintering of B4C and B4C-TiB2 composites: deformation
and failure mechanisms under quasistatic and dynamic loading, J. Eur. Ceram. Soc.
41 (6) (2021) 3321–3332, https://doi.org/10.1016/j.jeurceramsoc.2021.01.044.
[46] M. Taya, S. Hayashi, A.S. Kobayashi, H.S. Yoon, Toughening of a particulate
reinforced ceramic-matrix composite by thermal residual stress, J. Am. Ceram. Soc.
73 (5) (1990) 1382–1391, https://doi.org/10.1111/j.1151-2916.1990.tb05209.x.
[47] J.D. Clayton, R.B. Leavy, J. Knap, Phase field mechanics of residually stressed
ceramic composites, Philos. Mag. A 102 (19) (2022) 1891–1944, https://doi.org/
10.1080/14786435.2022.2086715.
[48] J. Tatami, K. Yasuda, Y. Matsuo, S. Kimura, Stochastic analysis on crack path of
polycrystalline ceramics based on the difference between the released energies in
crack propagation, J. Mater. Sci. 32 (1997) 2341–2346, https://doi.org/10.1023/
A:1018588620081.
[49] K.J. Lin, X. Zong, P.F. Sheng, S.Z. Zhao, Y.J. Qi, W.D. Zhang, S.H. Wu, Effects of
SmF3 addition on aluminum nitride ceramics via pressureless sintering, J. Eur.
Ceram. Soc. 43 (15) (2023) 6804–6814, https://doi.org/10.1016/j.
jeurceramsoc.2023.07.051.
[50] S. Bueno, M.H. Berger, R. Moreno, C. Baudín, Fracture behaviour of microcrackfree alumina–aluminium titanate ceramics with second phase nanoparticles at
alumina grain boundaries, J. Eur. Ceram. Soc. 28 (10) (2008) 1961–1971, https://
doi.org/10.1016/j.jeurceramsoc.2008.01.017.
[51] D.B. Marshall, Controlled surface flaws in ceramics: a comparison of Knoop and
Vickers indentation, J. Am. Ceram. Soc. 66 (2) (1983) 127–131, https://doi.org/
10.1111/j.1151-2916.1983.tb09989.x.
[52] Jr R.F.K, Rising fracture toughness from the bending strength of indented alumina
beams, J. Am. Ceram. Soc. 71 (5) (1988) 338–343, https://doi.org/10.1111/
j.1151-2916.1988.tb05051.x.
[53] N. Ramachandran, L.Y. Chao, D.K. Shetty, R-curve behavior and flaw insensitivity
of Ce-TZP/Al2O3 composite, J. Am. Ceram. Soc. 76 (4) (1993) 961–969, https://
doi.org/10.1111/j.1151-2916.1993.tb05320.x.
29641
0
You can add this document to your study collection(s)
Sign in Available only to authorized usersYou can add this document to your saved list
Sign in Available only to authorized users(For complaints, use another form )