Cu-Ni Welding Guidelines
1. Preparation Before Welding
•
Remove all contaminants (oil, grease, crayon, oxides) and preheat to remove moisture if necessary
•
Clean at least 25 mm from the edge of the weld area, use uncontaminated cleaning tools (use only for cu-ni) and
no carbon steel tools
•
Check the shielding gas container, and make sure the heater is on
•
Make sure the purging gas is running and sealed well
•
Check the welding gun
▪
Check the collet, make sure the airflow holes are not blocked or damaged
▪
Check that the gas cup is used for the gas flow that the welder is going to use to reduce the possibility of
turbulent airflow. Use a bigger cup size to reduce the potential of turbulence or reduce the gas flow
2. Fit-up
•
Use small and narrow tack with spacing closer than carbon steel (more tack than carbon steel)
3. During Welding
•
Use stringer beads. Because of the nature of the Cu-Ni sluggish weld pool, the welders tend to weave
•
Proper use of torch angle (150 recommended)
•
Make sure to follow all parameter written in the WPS
•
Clean every tack weld well
•
Clean every pass thoroughly before commencing the next pass
•
Limit the interpass to follow WPS
•
If possible, use a quarter welding sequence to reduce the interpass temperature.
2
4
3
1
4. After Welding
•
Clean the weld area of possible oxide formed during welding by uncontaminated non carbon steel brush
5. References
•
https://www.youtube.com/watch?v=t2JZYn819DQ&t=3s (1 Cleaning and Preparation for Welding of Copper
Nickel Alloy Part 1 of 5)
•
https://www.youtube.com/watch?v=abr7gMdAlkU (2 TIG Welding Copper Nickel Alloy Part 2 of 5)
•
https://www.youtube.com/watch?v=NBS7BF_iE_k&t=2s (3 Pipe Welding Copper Nickel Alloy Part 3 of 5)
•
https://www.copper.org/applications/marine/cuni/pdf/pub139.pdf (Copper-nickel Welding and Fabrication)