INTERNATIONAL STANDARD ISO 148-1 Third edition 2016-10-15 Metallic materials — Charpy pendulum impact test — Part 1: Test method Matériaux métalliques — Essai de flexion par choc sur éprouvette Charpy — Partie 1: Méthode d’essai Reference number ISO 148-1:2016(E) © ISO 2016 ISO 148-1:2016(E) COPYRIGHT PROTECTED DOCUMENT © ISO 2016, Published in Switzerland All rights reserved. Unless otherwise specified, no part o f this publication may be reproduced or utilized otherwise in any form or by any means, electronic or mechanical, including photocopying, or posting on the internet or an intranet, without prior written permission. Permission can be requested from either ISO at the address below or ISO’s member body in the country o f the requester. ISO copyright o ffice Ch. de Blandonnet 8 • CP 401 CH-1214 Vernier, Geneva, Switzerland Tel. +41 22 749 01 11 Fax +41 22 749 09 47 copyright@iso.org www.iso.org ii © ISO 2016 – All rights reserved ISO 148-1:2016(E) Contents Page Foreword ........................................................................................................................................................................................................................................ iv 1 Scope ................................................................................................................................................................................................................................. 1 2 Normative references ...................................................................................................................................................................................... 1 3 Terms and definitions ..................................................................................................................................................................................... 1 .............................................................................................................................................. 1 ....................................................................................................................................... 2 4 Symbols and abbreviated terms ........................................................................................................................................................... 2 5 Principles of the test......................................................................................................................................................................................... 3 6 Test pieces ................................................................................................................................................................................................................... 3 6.1 General ........................................................................................................................................................................................................... 3 ...................................................................................................................................................................................... 4 6.2.1 V-notch...................................................................................................................................................................................... 4 6.2.2 U-notch ..................................................................................................................................................................................... 4 6.3 Tolerance of the test pieces .......................................................................................................................................................... 4 6.4 Preparation of the test pieces..................................................................................................................................................... 4 6.5 Marking of the test pieces .............................................................................................................................................................. 4 7 Test equipment....................................................................................................................................................................................................... 4 7.1 General ........................................................................................................................................................................................................... 4 ........................................................................................................................................................ 5 7.3 Striker ............................................................................................................................................................................................................. 5 8 Test procedure ........................................................................................................................................................................................................ 5 8.1 General ........................................................................................................................................................................................................... 5 8.2 Friction measurement ...................................................................................................................................................................... 5 8.3 Test temperature ................................................................................................................................................................................... 6 8.4 Specimen transfer ................................................................................................................................................................................ 7 ....................................................................................................................................................... 7 8.6 Incomplete fracture ............................................................................................................................................................................ 7 8.7 Test piece jamming.............................................................................................................................................................................. 8 8.8 Post-fracture inspection.................................................................................................................................................................. 8 9 Test report................................................................................................................................................................................................................... 8 f ................................................................................................................................................................... 8 9.2 Optional information ......................................................................................................................................................................... 8 Annex A (informative) Self-centring tongs .................................................................................................................................................. 12 Annex B (informative) Lateral expansion..................................................................................................................................................... 13 Annex C (informative) Fracture appearance ............................................................................................................................................. 16 Annex D (informative) Absorbed energy vs. temperature curve and the transition temperature ... 19 Annex E (informative) Measurement uncertainty of an absorbed energy value, K.......................................... 21 Bibliography ............................................................................................................................................................................................................................. 29 3 .1 D efinitio ns p ertaining to energy 3 .2 D efinitio ns p ertaining to tes t p iece 6.2 N o tch geo metry 7.2 I ns tallatio n and verificatio n 8.5 E xceeding machine cap acity 9.1 M andato ry in o rmatio n © ISO 2016 – All rights reserved iii ISO 148-1:2016(E) Foreword ISO (the International Organization for Standardization) is a worldwide federation of national standards bodies (ISO member bodies). The work o f preparing International Standards is normally carried out through ISO technical committees. Each member body interested in a subject for which a technical committee has been established has the right to be represented on that committee. International organizations, governmental and non-governmental, in liaison with ISO, also take part in the work. ISO collaborates closely with the International Electrotechnical Commission (IEC) on all matters o f electrotechnical standardization. The procedures used to develop this document and those intended for its further maintenance are described in the ISO/IEC Directives, Part 1. In particular the different approval criteria needed for the di fferent types o f ISO documents should be noted. This document was dra fted in accordance with the editorial rules of the ISO/IEC Directives, Part 2 (see www.iso.org/directives). Attention is drawn to the possibility that some o f the elements o f this document may be the subject o f patent rights. ISO shall not be held responsible for identi fying any or all such patent rights. Details o f any patent rights identified during the development o f the document will be in the Introduction and/or on the ISO list of patent declarations received (see www.iso.org/patents). Any trade name used in this document is in formation given for the convenience o f users and does not constitute an endorsement. For an explanation on the meaning o f ISO specific terms and expressions related to con formity assessment, as well as information about ISO’s adherence to the World Trade Organization (WTO) principles in the Technical Barriers to Trade (TBT) see the following URL: www.iso.org/iso/foreword.html. The committee responsible for this document is ISO/TC 164, Mechanical testing ofmetals, Subcommittee SC 4, Toughness testing — Fracture (F), Pendulum (P), Tear (T). This third edition cancels and replaces the second edition (ISO 148-1:2009), which has been technically revised. ISO 148 consists of the following parts, under the general title Metallic materials — Charpy pendulum impact test: — Part 1: Test method — Part 2: Verification of testing machines — Part 3: Preparation and characterization of Charpy V-notch test pieces for indirect verification of pendulum impact machines iv © ISO 2016 – All rights reserved INTERNATIONAL STANDARD ISO 148-1:2016(E) Metallic materials — Charpy pendulum impact test — Part 1: Test method 1 Scope T h i s p a r t o f I S O 14 8 s p e ci fie s the C ha rp y ( V-no tch and U-no tch) p endu lu m i mp ac t te s t me tho d for de term i n i ng the energ y ab s orb e d i n a n i mp ac t te s t o f me ta l l ic materia l s . T h i s p a r t o f I S O 14 8 do e s no t cover i n s tru mente d i mp ac t te s ti ng , wh ich i s s p e c i fie d i n I S O 145 5 6 . Annexes B and C are based on ASTM E23 and are used with the permission of ASTM International, 100 Barr Harbor Drive, P.O. Box C700, West Conshohocken, PA 19428-2959, USA. 2 Normative references T he fol lowi ng re ference d do c u ments , i n whole or i n p ar t, are normatively re ference d i n th i s do c u ment and a re i nd i s p en s able for the appl ic ation o f th i s do c ument. For date d re ference s , on ly the e d ition cite d appl ie s . For u ndate d re ference s , the l ate s t e d ition o f the re ference d do c u ment (i nclud i ng any amendments) applies. ISO 148-2, Metallic materials — Charpy pendulum impact test — Part 2: Verification of testing machines ISO 286-1, Geometrical product specifications (GPS) — ISO code system for tolerances on linear sizes — Part 1: Basis of tolerances, deviations and fits 3 Terms and definitions For the pu r p o s e s o f th i s do c u ment, the fol lowi ng term s and defi n ition s apply. 3.1 Definitions pertaining to energy 3.1.1 initial potential energy potential energy Kp p o tenti a l energ y o f the p endu lu m ha m mer prior to its rele a s e for the i mp ac t te s t, a s de term i ne d by d i re c t veri fic ation 3.1.2 absorbed energy K energ y re qui re d to bre a k a te s t pie ce with a p endu lu m i mp ac t te s ti ng mach i ne, a fter corre c tion friction N o te 1 to entr y: T he le tter V or U i s u s e d to i nd ic ate the no tch ge ome tr y, th at i s: used as a subscript to indicate the radius of the striker, for example KV2 . for KV or KU. The number 2 or 8 is 3.1.3 nominal initial potential energy nominal energy KN energ y as s igne d b y the ma nu fac tu rer o f the p endu lu m i mp ac t te s ti ng mach i ne © ISO 2016 – All rights reserved 1 ISO 148-1:2016(E) 3.2 Definitions pertaining to test piece 3.2.1 width W distance between the notched face and the opposite face N o te 1 to entr y: S e e Figu re 1 . N o te 2 to entr y: I n pre viou s vers ion s o f the I S O 14 8 s er ie s ( p r io r to 2 016 ) , the d i s ta nce b e twe en the no tche d face a nd the op p o s ite face wa s s p e c i fie d a s “ height”. C h a n gi n g th i s d i men s ion to “width” m a ke s th i s p a r t o f I S O 14 8 con s i s tent with the ter m i no lo g y u s e d i n o ther I S O frac tu re s ta nd a rd s . 3.2.2 thickness B dimension perpendicular to the width and parallel to the notch N o te 1 to entr y: S e e Figu re 1 . N o te 2 to entr y: I n pre viou s vers ion s o f the I S O 14 8 s erie s ( p r ior to 2 016 ) , the d i men s io n p er p end ic u l a r to the width th at i s p a ra l lel to the no tch wa s s p e c i fie d a s “width”. C h a n gi n g th i s d i men s ion to “th ickne s s ” m a ke s th i s p a r t o f I S O 14 8 con s i s tent with the ter m i nolo g y u s e d i n o ther I S O frac tu re s ta nda rd s . 3.2.3 length L largest dimension perpendicular to the notch N o te 1 to entr y: S e e Figu re 1 . 4 Symbols and abbreviated terms T he s ymb ol s and de s ignation s appl ic able to th i s p ar t o f I S O 14 8 a re i nd ic ate d i n illustrated in Figure 2. Tables 1 and 2, and are Table 1 — Symbols and their unit and designation Symbol 2 Unit B α β1 mm ° J or ° β2 J or ° L LE K mm mm J K1 J or ° K2 J or ° KN Kp KV2 J or ° J J Designation thickness of test piece angle of fall of the pendulum angle of rise when the machine is operated in the normal manner without a test piece in position angle of rise when the machine is operated in the normal manner without a test piece in position and without resetting the indication mechanism length of test piece lateral expansion KV2 , KV8 , KU2 , KU8 f tries and the radius of the striking edge) ab s o rb e d energ y (e xp re s s e d a s , to identi y s p e c i fic no tch ge ome i nd ic ate d ab s o rb e d energ y when the m ach i ne i s op erate d i n the nor m a l m a n ner without a test piece in position i nd ic ate d ab s o rb e d energ y when the m ach i ne i s op erate d i n the nor m a l m a n ner without a test piece in position and without resetting the indication mechanism no m i n a l i n iti a l p o tenti a l energ y i n itia l p o tenti a l energ y ( p o tentia l energ y) ab s o rb e d energ y for a V-no tch te s t pie ce u s i n g a 2 m m s tr i ker © ISO 2016 – All rights reserved ISO 148-1:2016(E) Table 1 (continued) Symbol Unit Tt27 J J J N·m J J J % °C mm °C Tt50 %US °C Tt50 % SFA °C Tt0,9 °C KV8 KU2 KU8 M p p ’ pβ SFA Tt W 5 Designation ab s orb e d energ y fo r a V-no tch te s t p ie ce u s i ng a 8 m m s tr i ker ab s orb e d energ y fo r a U-no tch te s t p ie ce u s i n g a 2 m m s tr i ker ab s orb e d energ y fo r a U-no tch te s t p ie ce u s i n g a n 8 m m s tr i ker moment equal to the product F·l2 ab s orb e d energ y lo s s c au s e d b y p oi nter fric tio n ab s orb e d energ y lo s s c au s e d b y b e a r i n g fric tio n a nd a i r re s i s ta nce cor re c tion o f ab s orb e d energ y lo s s e s fo r a n a n gle o f r i s e shear fracture appearance transition temperature width of test piece β tra n s ition temp eratu re de fi ne d at a s p e c i fic va lue o f ab s o rb e d energ y; for example, 27 J tra n s ition temp eratu re de fi ne d at a p a r tic u l a r p ercentage o f the ab s orb e d energ y o f the up p er s hel f; for e xa mp le , 5 0 % tra n s ition temp eratu re de fi ne d at a p a r tic u l a r p rop o r tion o f s he a r frac tu re; for example, 50 % tra n s ition temp eratu re de fi ne d at a p a r tic u l a r a mou nt o f l atera l e x p a n s ion; for example, 0,9 mm Principles of the test This test consists of breaking a notched test piece with a single blow from a swinging pendulum, under Clauses 6, 7 and 8 is located in the middle between two supports, opposite to the location which is impacted in the test. the cond ition s defi ne d i n . T he no tch i n the te s t pie ce h as a s p e ci fie d ge ome tr y a nd T he energ y ab s orb e d i n the i mp ac t te s t, the latera l exp an s ion and the she a r frac tu re app e ara nce are norma l ly de term i ne d . B e c au s e the i mp ac t va lue s o f ma ny me ta l l ic materia l s va r y with temp eratu re, te s ts s ha l l b e c arrie d out at a s p e ci fie d temp eratu re . When th i s temp eratu re i s o ther th an a mbient, the te s t pie ce sh a l l b e he ate d or cooled to that temperature, under controlled conditions. T he C har p y p endu lu m i mp ac t te s t i s o ften u s e d i n routi ne, h igh-th roughput p a s s/fai l accep ta nce te s ts i n i ndu s tria l s e tti ngs . For the s e te s ts , it may no t b e i mp or tant whe ther the te s t s a mple i s comple tely broken, p ar ti a l ly broken, or s i mply pla s tica l ly de forme d and d ragge d th rough the a nvi l s . I n re s e a rch, de s ign, or ac adem ic s e tti ngs , the me a s u re d energ y va lue s a re s tud ie d i n more de tai l, i n wh ich c as e it c an b e h igh ly relevant whe ther the s a mp le i s broken or no t. I t i s i mp or tant to no te th at no t a l l C har py p endu lu m i mp ac t te s t re s u lts c an b e d i re c tly comp are d . For example, the test can be performed with hammers having strikers with different radii, or with different test piece shapes. Tests performed with different strikers can give different results,[7] and test results ob ta i ne d with d i fferently sh ap e d te s t pie ce s c an as wel l . T h i s i s why no t on ly the ad herence to I S O 14 8 but a l s o a cle ar a nd comp le te rep or ti ng o f the typ e o f i n s tru ment, the te s t pie ce and the de tai l s o f the p o s t-te s t te s t pie ce s are cruc ia l for comp a rabi l ity o f re s u lts . 6 Test pieces 6.1 General The standard test piece shall be 55 mm long and of square section, with 10 mm sides. In the centre of the length, there shall be either a V-notch or a U-notch, as described in 6.2.1 and 6.2.2 , re s p e c tively. © ISO 2016 – All rights reserved 3 ISO 148-1:2016(E) If the standard test piece cannot be obtained from the material, one of the subsize test pieces, having a thickness of 7,5 mm, 5 mm or 2,5 mm (see Figure 2 and Table 2 f ) , sh a l l b e u s e d , i NO TE 1 no t o ther wi s e s p e ci fie d . D i re c t comp a r i s o n o f re s u lts i s on l y o f s ign i fic a nce when m ade b e twe en te s t p ie ce s o f the s a me for m and dimensions. NOTE 2 For low energies, the use of shims to better position subsize test pieces relative to the centre of important. Shims can be placed on or under the test piece supports, with the result that the mid-thickness of another means. s tr i ke i s i mp o r ta nt to avo id e xce s s energ y ab s or p tio n b y the p endu lu m . For h igh energie s , th i s m ight no t b e a s the s p e c i men i s 5 m m ab ove the 10 m m s upp or ts . S h i m s c a n b e temp ora r i l y fi xe d to the s upp or ts u s i ng tap e o r When a he at-tre ate d materi a l i s b ei ng eva luate d, the te s t pie ce sha l l b e fi n i sh-mach i ne d a nd no tche d a fter the fi na l he at tre atment, u n le s s it c an b e demon s trate d th at mach i n i ng b e fore he at tre atment do e s not affect test results. 6.2 Notch geometry T he no tch s ha l l b e c are fu l ly prep are d s o that the ro o t rad iu s o f the no tch i s fre e o f mach i n i ng marks wh ich cou ld a ffe c t the ab s orb e d energ y. T he plane o f s ym me tr y o f the no tch s ha l l b e p er p end ic u la r to the longitud i na l a xi s o f the te s t pie ce (see Figure 2). 6.2.1 V-notch The V-notch shall have an included angle of 45°, a depth of 2 mm and a root radius of 0,25 mm [see Figure 2 a) and Table 2]. 6.2.2 U-notch T he U-no tch s ha l l have a dep th o f 5 [see Figure 2 b) and Table 2]. m m (u n le s s o ther wi s e s p e c i fie d) and a ro o t rad iu s 6.3 Tolerance of the test pieces T he tolerance s on the s p e c i fie d te s t pie ce and no tch d i men s ion s are shown i n of 1 mm Figure 2 and Table 2. 6.4 Preparation of the test pieces P rep aration s ha l l b e exe c ute d i n s uch a way th at any a lteration o f the te s t pie ce, heating or cold working, is minimized. for example due to 6.5 Marking of the test pieces T he te s t pie ce may b e marke d on any face no t i n contac t with s upp or ts , anvi l s or s tri ker a nd at a p o s ition where pla s tic de formation and s ur face d i s conti nu itie s c au s e d by ma rki ng do no t a ffe c t the ab s orb e d energ y (s e e 8.8). 7 Test equipment 7.1 General The measurements of the instrument and test piece details shall be traceable to national or international standards. Equipment used for measurements shall be calibrated within suitable intervals. 4 © ISO 2016 – All rights reserved ISO 148-1:2016(E) 7 . 2 I n s t a l l a t i o n a n d v e r i f i c a t i o n T he te s ti ng mach i ne sh a l l b e i n s ta l le d a nd veri fie d i n accord ance with I S O 14 8 -2 . 7.3 Striker T he s tri ker ge ome tr y s ha l l b e s p e c i fie d as b ei ng either the 2 m m s tri ker or the 8 m m s tri ker. I t i s recommended that the radius on the striker be shown as a subscript as follows: KV2 or KV8 and KU2 or KU8 . Re ference s ha l l b e made to the pro duc t s p e c i fic ation for s tri ker ge ome tr y gu idance . NOTE Tests carried out with 2 mm and 8 mm strikers can give different results. [7] 8 Test procedure 8.1 General T he te s t pie ce s ha l l l ie s quarely agai n s t the a nvi l s o f the te s ti ng mach i ne, with the plane o f s ym me tr y o f the no tch with i n 0 , 5 m m o f the m id-pl ane b e twe en the a nvi l s . I t sha l l b e s truck b y the s tri ker i n the plane o f s ym me tr y o f the no tch and on the s ide opp o s ite the no tch (s e e 8.2 Figure 1). Friction measurement T he energ y ab s orb e d b y fric tion sha l l b e che cke d on ever y te s ti ng day prior to the fi rs t te s t. T he fric tion lo s s e s may b e e s ti mate d as e xpl ai ne d b elow, but o ther me tho d s may a l s o b e appl ie d . NO TE T he energ y ab s orb e d b y fr ic tion i nclude s , but i s no t l i m ite d to, a i r re s i s tance, b e a ri ng fric tion a nd the fr ic tion o f the i nd ic ati ng p oi nter. I nc re a s e s i n fr ic tion on a mach i ne c a n i n fluence the me as u re o f ab s orb e d energ y. 8.2.1 To determine the lo s s caus ed by p o inter frictio n the machine is o p erated in the no rmal manner, but without a test piece in position, and the angle of rise, β1 K1 , is noted. A second test is then carried out without resetting the indication pointer and the new angle of rise, β2 reading, K2 , is noted. Thus, the loss due to friction in the indicating pointer during the rise is equal to p = M(cos β1 β2 ) (1) , o r energy reading, , o r energy − co s when the scale is graduated in degrees, or p = K1 K2 − (2) when the s c a le i s graduate d i n energ y un its . NO TE 8.2.2 Fo r m ach i ne s without a p o i nter, th i s fr ic tio n me a s u rement i s no t ne ce s s a r y. The p ro cedure to determine the lo s s es caus ed by b earing frictio n and air res is tance fo r o ne hal f swing is as follows. After determining β2 or K2 , the pendulum is returned to its initial position. Without resetting the indicating mechanism, release the pendulum without shock and vibration and permit it to swing 10 half swings. After the pendulum starts its 11th half swing, move the indicating mechanism to about © ISO 2016 – All rights reserved 5 ISO 148-1:2016(E) 5 % o f the s c a le -range c ap ac ity a nd re cord the va lue as resistance for one half swing are equal to p M(cos β3 β2 ) ′ = 1 /10 β3 or K3 . T he lo s s e s b y b e a ri ng fric tion a nd ai r (3) − co s when the scale is graduated in degrees, or p K3 K2 ) ′ = 1 /10 ( (4) − when the s c a le i s graduate d i n energ y u n its . The number of swings can be changed at the discretion of machine users, and p’ should be corrected on account of the applied number of swings. NOTE 1 If it is required to take into account these losses in an actual test giving an angle of rise, β , the qu a ntity c a n b e s ub trac te d fro m the va lue o f the ab s orb e d energ y. pβ = p β β1 + p′ α +β Because β1 and β2 reduced to: pβ = p β α + p′ (5) α + β2 a re ne arly e qua l to , the angle of fall, for practical purposes Formula (5) can be α α +β (6) 2α For mach i ne s graduate d i n energ y u n its , the va lue o f ( β = a rcco s[1 − 1 /M KP − KT )] β can be calculated as follows: (7) The total friction loss, p + p bearings shall be cleaned or replaced. ′, s o me as u re d , s ha l l no t exce e d 0 , 5 % o f the nom i na l energ y, KN . If it does, a nd it i s no t p o s s ible to bri ng the fric tion lo s s with i n the tolera nce b y re duc i ng the p oi nter fric tion, the 8.3 8.3.1 Test temperature Unles s o therwis e s p ecified, tes ts s hall b e carried o ut at 2 3 °C ± 5 °C (amb ient temp erature) . I f a temp erature is s p ecified, the tes t p iece s hall b e co nditio ned to a temp erature within ± 2 °C . 8.3.2 For conditioning (heating or cooling) using a liquid medium, the test piece shall be positioned in a co ntainer o n a grid that is at leas t 2 5 mm ab ove the b o tto m o f the co ntainer and covered by at leas t 2 5 mm o f liquid, and b e at leas t 1 0 mm fro m the s ides o f the co ntainer. The medium s hall b e co ns tantly agitated and b ro ught to the s p ecified temp erature by any co nvenient metho d. The device us ed to measure the temperature of the medium should be placed in the centre of the group of test pieces. The temp erature o f the medium s hall b e held at the s p ecified temp erature within ± 1 °C fo r at leas t 5 min. NO TE W hen a l iqu id me d iu m is ne a r its b o i l i ng p o i nt, e vap orative co o l i ng c a n d ra m atic a l l y lower the temperature of the test piece during the interval between removal from the liquid and fracture. [8] 8.3.3 For conditioning (heating or cooling) using a gaseous medium, the test piece shall be positioned in a chamb er at leas t 5 0 mm fro m the neares t s urface. I ndividual tes t p ieces s hall b e s ep arated by at leas t 1 0 mm. The medium s hall b e co ns tantly circulated and b ro ught to the s p ecified temp erature by any co nvenient metho d. The device us ed to meas ure the temp erature o f the medium s ho uld b e p laced in the centre of the group of test pieces. The temperature of the gaseous medium shall be held at the for testing. s p ecified temp erature within ± 1 °C fo r at leas t 3 0 min b e fo re the tes t p iece is removed fro m the medium 6 © ISO 2016 – All rights reserved ISO 148-1:2016(E) 8.3.4 Other methods for heating or cooling are allowed, if the other pertinent requirements of 8.3 are ulfilled. f 8.4 Specimen transfer When testing is performed at other than ambient temperature, not more than 5 s shall elapse between the time the test piece is removed from the heating or cooling medium and the time it is impacted by the striker. An exception is made if the difference between the ambient or instrument temperature and the test piece temperature is less than 25 °C, in which case the time for specimen transfer shall be less than 10 s. The trans fer device shall be designed and used in such a way that the temperature o f the test piece is maintained within the permitted temperature range. The parts of the device in contact with the specimen during transfer from the medium to the machine shall be conditioned with the specimens. Care should be taken to ensure that the device used to centre the test piece on the anvils does not cause the fractured ends o f low-energy, high-strength test pieces to rebound o ff the device into the pendulum. This pendulum/test piece interaction results in erroneously high indicated energy. It has been shown that clearance between the end o f a test piece in the test position and the centring device, or a fixed portion of the machine, shall be equal to or greater than 13 mm to avoid the ends of the test pieces rebounding into the pendulum during the test. NOTE Self-centring tongs, similar to those shown in Annex A for V-notched test pieces, are often used to transfer the test piece from the temperature-conditioning medium to the proper test position. Tongs of this nature eliminate potential clearance problems due to interference between the fractured specimen halves and a fixed centring device. 8.5 Exceeding machine capacity The absorbed energy, K, should not exceed 80 % o f the initial potential energy, Kp . If the absorbed energy exceeds this value, the absorbed energy shall be reported as approximate and it shall be noted in the test report as exceeding 80 % o f the machine capacity. NOTE Ideally, an impact test would be conducted at a constant impact velocity. In a pendulum-type test, the velocity decreases as the fracture progresses. For specimens with impact energies approaching the capacity o f the pendulum, the velocity o f the pendulum decreases during fracture to the point that accurate impact energies are no longer obtained. 8.6 Incomplete fracture Test pieces do not always break into two pieces during the test. For material acceptance testing, it is not required to report information concerning incomplete fracture. For tests, other than material acceptance testing, it is required that unbroken test pieces are reported. NOTE 1 In the case where individual specimens are not identified within test records, the group can be identified as broken or unbroken. NOTE 2 A test piece that is not fully separated in two hal f test pieces upon impact can be considered broken i f the two halves can be separated by pushing the hinged halves together without the aid o f mechanical tools and without fatiguing the specimen. NOTE 3 A material acceptance test is a test which is used to asses a minimum acceptance requirement. © ISO 2016 – All rights reserved 7 ISO 148-1:2016(E) 8.7 Test piece jamming I f a te s t pie ce j am s i n the mach i ne, the re s u lts s ha l l b e d i s re garde d a nd the mach i ne thorough ly che cke d for damage that would affect its state of calibration. NOTE Jamming occurs when a broken test piece is caught between moving and non-moving parts of the ff f strike marks, because jamming is associated with a pair of opposing marks on the specimen. te s ti n g m ach i ne . I t c a n re s u lt i n s ign i fic a nt energ y ab s o r p tion . Ja m m i n g c a n b e d i erenti ate d ro m s e cond a r y 8.8 Post-fracture inspection I f p o s t- frac ture i n s p e c tion shows that a ny p or tion o f the te s t s p e c i men identi fic ation marki ng i s i n a p or tion o f the te s t pie ce wh ich i s vi s ibly de forme d , the te s t re s u lt m ight no t b e repre s entative o f the material and this shall be noted in the test report. 9 Test report 9.1 Mandatory information T he te s t rep or t s ha l l contai n the fol lowi ng i n formation or, when agre e d b y the c u s tomer, it s ha l l b e p o s s ible to re trieve th i s i n formation b a s e d on a trace able co d i ng o f the te s t rep or t b y the te s t lab orator y: a) re ference to th i s p ar t o f I S O 14 8 , i . e . I S O 14 8 -1 ; b) identi fic ation o f the te s t pie ce (e . g. typ e o f s te el and c a s t numb er) ; c) s i z e o f the te s t pie ce, i f o ther tha n the s tanda rd te s t pie ce; d) temp eratu re o f the te s t or the cond itioni ng temp eratu re o f the te s t s p e ci men s; e) ab s orb e d energ y, f) whe ther the s p e c i men, or the maj ority o f s p e ci men s i n a group o f s p e c i men s were broken (no t KV2 , KV8 , KU2 , or KU8 , as appropriate; re qui re d for materia l accep ta nce te s ts) ; g) any abnorma l itie s that cou ld h ave a ffe c te d the te s t. 9.2 Optional information T he te s t rep or t may op tiona l ly i nclude, i n add ition to the i n formation i n a) te s t pie ce orientation (s e e I S O 3 78 5 ) ; b) i n iti a l p o tentia l energ y o f the te s ti ng mach i ne, i n j ou le s; c) lateral expansion (see Annex B d) shear fracture appearance (see Annex C 9.1: ); ); D.1 e) ab s orb e d energ y/temp erature c u r ve (s e e ); f) latera l e xp an s ion/temp eratu re c u r ve; g) s he ar frac tu re app e arance/temp eratu re c ur ve; h) transition temperature(s) and the criteria used for its (their) determination (see D.2 i) nu mb er o f te s t pie ce s wh ich were no t comple tely broken i n the te s t; j) date (month and ye ar) o f the mo s t re cent fu l l d i re c t a nd i nd i re c t veri fic ation s; k) me a s u rement u ncer tai nty o f the ab s orb e d energ y (s e e 8 ); Annex E). © ISO 2016 – All rights reserved ISO 148-1:2016(E) 8 Key 1 2 3 4 5 6 7 8 9 F anvil standardized test piece test piece supports shroud width of test piece, W length of test piece, L thickness of test piece, B centre of strike direction of pendulum swing i g u r e 1 — T e s t p i e c e t e r m i n o l o g y s h o w i n g c o n f i g u r a t i o n o f t e s t p i e c e s u p p o r t s a n d a n v i l s of a pendulum impact testing machine © ISO 2016 – All rights reserved 9 ISO 148-1:2016(E) L a) V-notch geometry L b) U-notch geometry NO TE Fo r the s ymb ol s L , W, B and the numbers 1 to 5, refer to Table 2. Figure 2 — Charpy pendulum impact test piece 10 © ISO 2016 – All rights reserved ISO 148-1:2016(E) T a b l e 2 — T o l e r a n c e s o n s p e c i f i e d t e s t p i e c e d i m e n s i o n s V-notch test piece U-notch test piece Symbol Machining tolerance Designation and Nominal Machining tolerance Nominal Tolerance dimension Tolerance no. dimension class a class a Length L 55 mm js15 55 mm js15 Width W 10 mm js12 10 mm js13 c Thickness B 10 mm js13 10 mm js13 — standard test 10 mm js13 10 mm js13 piece 7,5 mm js13 7,5 mm — — subsize test piece 5 mm js12 5 mm — — subsize test piece 2,5 mm js12 — — — — subsize test piece Angle of notch 1 45° — — — — Ligament 2 8 mm js12 5 mm js13 Notch radius 3 0,25 mm — 1 mm js12 d d Notch position 4 27,5 mm js15 27,5 mm js15 (centering) Angle between plane 90° — 90° — f f and longitudinal axis of test piece Angle between 5 90° — 90° — adjacent longitudinal faces of test piece Surface roughnessb NA ±0,60 mm ±0,60 mm ± 0 , 0 75 m m ± 0 ,1 1 m m ± 0 ,1 1 m m ± 0 ,1 1 m m ± 0 ,1 1 m m ± 0 ,1 1 m m ± 0 ,1 1 m m ± 0 ,1 1 m m ±0,06 mm ±0,06 mm ±0,05 mm ±2 ° o s ym me tr y o ±0,09 mm ±0 ,02 5 mm ±0,07 mm ± 0 ,42 m m ± 0 ,42 m m ±2 ° ±2 ° ±2 ° ±2 ° no tch < 5 μm a b c d ± 0 , 0 75 m m < 5 μm In accordance with ISO 286-1. The test pieces shall have a surface roughness better than Ra 5 µm except for the ends. I f a no ther th ickne s s (2 m m o r 3 m m) i s s p e c i fie d , the co r re s p o nd i n g to lera nce s s h a l l a l s o b e s p e c i fie d . Fo r m ach i ne s with auto m atic p o s itio n i n g o f the te s t p ie ce , i t i s re co m me nde d th at the to lera nce b e ta ke n a s ± 0 ,1 6 5 m m i n s te ad o f ± 0 , 42 m m . © ISO 2016 – All rights reserved 11 ISO 148-1:2016(E) Annex A (informative) Self-centring tongs Tongs similar to the example shown in Figure A.1 position it in the pendulum impact testing machine. are o ften u s e d to tran s fer the te s t pie ce and prop erly a Dimensions in millimetres Steel pieces silver soldered to tongs parallel to each other. Specimen thickness 10 5 3 A 1,60 to 1,70 0,74 to 0,80 0,45 to 0,51 B 1,52 to 1,65 0,69 to 0,81 0,36 to 0,48 Figure A.1 — Centring tongs for V-notched Charpy specimens 12 © ISO 2016 – All rights reserved ISO 148-1:2016(E) Annex B (informative) Lateral expansion B.1 General A measure o f the ability o f the material to resist fracture when subjected to triaxial stresses, such as those at the root o f the notch in a Charpy test piece, is the amount o f de formation that occurs at this location. The de formation in this case is contraction. Because o f the di fficulties in measuring this deformation, even after fracture, the expansion that occurs at the opposite end of the fracture plane is customarily measured and used as a proxy for the contraction. B.2 Procedure The method of measuring lateral expansion should take into account the fact that the fracture plane seldom bisects the point of maximum expansion on both sides of a test piece. One half of a broken test piece might include the maximum expansion for both sides, one side only, or neither. The techniques used should therefore provide an expansion value, equal to the sum of the higher of the two values obtained for each side, by measuring the two halves separately. The amount o f expansion on each side o f each hal f shall be measured relative to the plane defined by the unde formed portion o f the side o f the test piece (see Figure B.1). Contact and non-contact methods can be used for these measurements. Lateral expansion may be measured by using a gauge similar to that shown in Figures B.2 and B.3. Measure the two broken halves individually. First, however, check the sides perpendicular to the notch to ensure that no burrs were formed on these sides during impact testing; i f such burrs exist, they shall be removed, for example by rubbing with an emery cloth, making sure that the protrusions to be measured are not rubbed during the removal of the burr. Next, place the half-specimens together so that the sur faces originally opposite the notch are facing one another. Take one o f the hal f-specimens (see Figure B.1) and press it firmly against the reference supports, with the protrusions against the gauge anvil. Note the reading, and then repeat this step with the other half-specimen (see Figure B.1), ensuring that the same side is measured. The larger of the two values is the expansion of that side of the test piece. Repeat this procedure to measure the protrusions on the opposite side, and then add the larger values obtained for each side. For example if A1 > A2 and A3 = A4, consequently LE = A1 + (A3 or A4). If A1 > A 2 and A 3 > A4 , consequently, LE = A1 + A 3 . I f one or more protrusions o f a test piece have been damaged by contacting the anvil, machine mounting surface, etc., the test piece shall not be measured and the condition shall be indicated in the test report. © ISO 2016 – All rights reserved 13 ISO 148-1:2016(E) A2 B A4 A1 B A3 Key 1 2 side one of fractured test piece side two of fractured test piece B thickness of test piece, mm A 1 , A 2 , A 3 , A 4, distance measured, mm Figure B.1 — Halves of broken Charpy V-notched impact specimen, illustrating the measurement of lateral expansion Figure B.2 — Lateral expansion gauge for Charpy specimens showing both halves of a Charpy specimens being measured on one side, rather than each half individually 14 © ISO 2016 – All rights reserved ISO 148-1:2016(E) Dimensions in millimetres Key 1 2 3 4 a b c pad made of rubber indicator, 10 mm range, graduations in 1/100 mm base plate made of stainless steel or chrome-plated steel dial mount made of stainless steel or chrome-plated steel Fo r 1 /4- 2 0 UN C s crew with 7 /8 ” lo ng s o cket head to mo unt the indicato r. For M6 × 1 screw with 25 mm socket head. Lap at as s emb ly. Figure B.3 — Assembly and details for lateral expansion gauge © ISO 2016 – All rights reserved 15 ISO 148-1:2016(E) Annex C (informative) Fracture appearance C.1 General T he frac ture s u r face o f C h ar py te s t pie ce s i s o ften rate d b y the p ercentage o f she ar frac tu re wh ich T he frac tu re s ur face o f mo s t C har p y s p e c i men s e xh ibits a m i x tu re o f s he a r and flat frac tu re region s . occurs. The greater the percentage of shear fracture, the greater the notch toughness of the material. T he she ar region s are as s u me d to b e fu l ly duc ti le, but the flat frac tu re region s c an b e duc ti le, brittle, or a combi nation o f the s e frac tu re mo de s . B e c au s e the rati ng i s ex tremely s ubj e c tive, it i s re com mende d that it i s no t to b e u s e d i n s p e ci fic ation s . NO TE T he ter m fib rou s - frac tu re ap p e a ra nce i s o ften u s e d a s a s ynonym for s he a r frac tu re ap p e a ra nce . T he term s cle avage frac tu re ap p e a ra nce a nd c r ys ta l l i n ity a re o ften u s e d to e xp re s s the op p o s ite o f s he a r frac tu re . C.2 Procedures T he p ercentage o f s he ar frac tu re i s com mon ly de term i ne d b y any one o f the fol lowi ng me tho d s: a) me a s u ri ng the leng th a nd width o f the cle avage p or tion (the “sh i ny” p or tion) o f the flat frac tu re region, as given in Figure C.1, and determining the percent shear from Table C.1 b) comparing the appearance of the fracture of the test piece with a fracture appearance chart, such as that given in Figure C.2 ; ; c) magn i fyi ng the frac tu re s u r face and comp ari ng it to a pre c a l ibrate d overlay char t, or me as u ri ng the p er cent cle avage frac ture b y me an s o f a p lan i me ter, then c a lc u l ati ng p er cent she a r frac tu re (a s 10 0 % cle avage frac tu re) ; d) pho to graph i ng the frac tu re s u r face at a s uitable magn i fic ation a nd me a s u ri ng the p er cent cle avage frac tu re b y me an s o f a pl an i me ter, then c a lc u lati ng p er cent she ar frac tu re (as 10 0 % cle avage frac tu re) ; e) 16 me a s u ri ng the p er cent s he ar frac tu re b y i mage ana lys i s te ch nique s . © ISO 2016 – All rights reserved ISO 148-1:2016(E) Key 1 notch 2 cleavage area (brittle) 3 shear area (dull) A dimension measured to estimate the cleavage area B dimension measured to estimate the cleavage area NOTE 1 Measure dimensions A and B to the nearest 0,5 mm. NOTE 2 Determine the per cent shear fracture using Table C.1. Figure C.1 — Determination of per cent shear fracture Table C.1 — Per cent shear for measurements in millimetres A mm mm 1,0 1,5 2,0 2,5 3,0 3,5 4,0 4,5 5,0 5,5 6,0 6,5 7,0 7,5 8,0 8,5 9,0 9,5 10 B 1,0 1,5 2,0 2,5 3,0 3,5 4,0 4,5 5,0 5,5 6,0 6,5 7,0 7,5 8,0 Per cent shear 99 98 98 97 96 96 95 94 94 93 92 92 91 91 90 89 89 88 88 98 97 96 95 94 93 92 92 91 90 89 88 87 86 85 84 83 82 81 98 96 95 94 92 91 90 89 88 86 85 84 82 81 80 79 77 76 75 97 95 94 92 91 89 88 86 84 83 81 80 78 77 75 73 72 70 69 96 94 92 91 89 87 85 83 81 79 77 76 74 72 70 68 66 64 62 96 93 91 89 87 85 82 80 78 76 74 72 69 67 65 63 61 58 56 95 92 90 88 85 82 80 77 75 72 70 67 65 62 60 57 55 52 50 94 92 89 86 83 80 77 75 72 69 66 63 61 58 55 52 49 46 44 94 91 88 85 81 78 75 72 69 66 62 59 56 53 50 47 44 41 37 93 90 86 83 79 76 72 69 66 62 59 55 52 48 45 42 38 35 31 92 89 85 81 77 74 70 66 62 59 55 51 47 44 40 36 33 29 25 92 88 84 80 76 72 67 63 59 55 51 47 43 39 35 31 27 23 19 91 87 82 78 74 69 65 61 56 52 47 43 39 34 30 26 21 17 12 91 86 81 77 72 67 62 58 53 48 44 39 34 30 25 20 16 11 6 90 85 80 75 70 65 60 55 50 45 40 35 30 25 20 15 10 5 0 NOTE 100 % shear shall be reported when A and B are zero. © ISO 2016 – All rights reserved 17 ISO 148-1:2016(E) a) Fracture appearance charts and per cent shear fracture comparator b) Guide for estimating fracture appearance Figure C.2 — Fracture appearance 18 © ISO 2016 – All rights reserved ISO 148-1:2016(E) Annex D (informative) Absorbed energy vs. temperature curve and the transition temperature D.1 Absorbed energy/temperature curve K/T T he ab s orb e d energ y/temp eratu re c u r ve ( te s t temp eratu re c u r ve) s hows the energ y ab s orb e d a s a for a given typ e o f te s t pie ce (s e e Figure D.1 fu nc tion o f the ) . I n genera l, the c u r ve i s ob tai ne d b y d rawi ng a fitte d c u r ve th rough the i nd ividua l va lue s . T he shap e o f the c u r ve and the s c atter o f the te s t va lue s a re dep endent on the materi a l, the s p e c i men sh ap e and the i mp ac t velo c ity. I n the c a s e o f a c u r ve with a ductile-to-brittle transition zone, a distinction is made between the upper-shelf zone, transition zone and the lower-shelf zone. Key T temperature K ab s o rb ed energy 1 upper-shelf zone 2 transition zone 3 lower-shelf zone NOTE Transition curves for shear fracture area and for lateral expansion are also common, but are not shown here. Figure D.1 — Absorbed energy/temperature curve shown schematically D.2 Transition temperatures The transition temperature, Tt, characterizes the position of the steep rise in the absorbed energ y/temp eratu re c u r ve . Si nce the s te ep ri s e u s ua l ly ex tend s over a fai rly wide temp eratu re range, © ISO 2016 – All rights reserved 19 ISO 1 48-1 : 2 01 6(E) there c an b e no genera l ly appl ic able defi n ition o f the tra n s ition temp eratu re . T he have, among others, been found useful for determining the transition temperature: a) Tt27 f KV8 b) Tt50 %US f f , corre s p ond i ng to a s p e c i fic va lue o ab s orb e d energ y, e . g. , corre s p ond i ng to a p ar tic u la r p ercentage o fol lowi ng criteri a = 2 7 J; the ab s orb e d energ y o the upp er- shel f va lue, e . g. 5 0 %; c) Tt50 %SFA f f d) Tt0,9, corresponding to a particular amount of lateral expansion, e.g. 0,9 mm. , corre s p ond i ng to a p ar tic u la r prop or tion o s he ar rac tu re , e . g. 5 0 %; T he me tho d u s e d to defi ne the tran s ition temp eratu re shou ld b e s p e ci fie d i n the pro duc t s tandard or s p e c i fic ation, or e s tabl i she d b y agre ement. NO TE 20 T he mo s t com mon l y u s e d fitti ng mo del fo r tra n s ition c u r ve s i s the hyp erb ol ic ta n gent fitti ng mo del . © ISO 2016 – All rights reserved ISO 148-1:2016(E) Annex E (informative) Measurement uncertainty of an absorbed energy value, K E.1 Symbols and units T he s ymb ol s and u n its u s e d i n th i s a n nex are given i n where the letter V or U Symbol BV Table E.1. KV i s u s e d for e xample pur p o s e s on ly, i nd ic ate s no tch ge ome tr y. Table E.1 — Symbols and units Unit Definition J bias of the pendulum impact testing machine, as determined through indire c t ver i fic ation k KV J J J J KV KVR KV V n J J J J r sx Tx u ( KV ) U( KV) u (r) uT uV J ab s o rb e d energ y a s me a s u re d i n accord a nce with th i s I nter n ation a l S ta nd ard on V-notched sample reported average KV value of a set of samples from a test material cer ti fie d KV - va lue o f the re ference m ater i a l u s e d i n the i nd i re c t ver i fic atio n mean KV f f f number of tested samples instrument scale resolution standard deviation of the values obtained on the n test samples error of measured KV value due to temperature effects va lue o the re erence te s t pie ce s te s te d s ta nd a rd u ncer ta i nty o f KV e x p a nde d u ncer ta i nty o f KV o r i nd i re c t ver i fic atio n with a con fidence le vel o f ab out 9 5 % s ta nd a rd u ncer ta i nty due to m ach i ne re s olutio n K u ( x) J J x J ν coverage factor KV νV vx © ISO 2016 – All rights reserved s ta nd a rd u ncer ta i nty o f the te s t temp eratu re s ta nd a rd u ncer ta i nty o f the i nd i re c t veri fic ation re s u lt s ta nd a rd u ncer ta i nty o f x observed average KV value of a set of n samples from a test material without correction for bias degrees of freedom corresponding with u ( KV ) degrees of freedom corresponding with uV degrees of freedom corresponding with u ( x ) 21 ISO 148-1:2016(E) E.2 Determination of measurement uncertainty E.2.1 General This Annex specifies a robust method for determining the uncertainty, u ( KV ) , associated with the mean absorbed energy, KV , of a set of specimens of a test material. Other methods of assessing u ( KV ) can be developed and are acceptable, i f they meet the requirements o f the GUM. [4] This approach requires input from the “indirect verification” o f the Charpy pendulum impact testing machine, which is a normative method of assessing the performance of the instrument with reference test pieces (see ISO 148-2). NOTE 1 The ISO 148 series requires Charpy pendulum impact testing machines to success fully meet the requirements for both indirect and direct verification. The latter consists o f a check o f all individual geometric and mechanical requirements imposed on the construction of the instrument (see ISO 148-2). The roles o f direct and indirect verification in the metrological traceability chain o f Charpy measurements are given in Figure E.1 . The chain starts at the international level with the definition of the measurand, KV, or absorbed energy, in the standard procedures described in the ISO 148 series. Global comparability relies on international comparisons o f Charpy re ference machines and o f the certified values o f the certified re ference test pieces produced by national or international bodies using sets of reference machines. Calibration laboratories use the certified re ference test pieces to veri fy their re ference machine and can use their pendulum to characterize and produce re ference test pieces. At the user level, Charpy test laboratories can veri fy their pendulum with re ference test pieces to obtain reliable KV values. NOTE 2 Users can choose to acquire certified re ference test pieces from national or international organizations, by-passing the calibration laboratory level. NOTE 3 For additional in formation on the di fference between certified re ference test pieces and re ference test pieces, see ISO 148-3:2016, Annex A. E.2.2 Uncertainty disclaimer Measurement uncertainty analysis is use ful in identi fying major sources o f inconsistencies in measured results. Product standards and material property databases based on this part o f ISO 148 have an inherent contribution from measurement uncertainty. It is there fore inappropriate to apply further adjustments for measurement uncertainty and thereby risk a product which fails compliance. For this reason, the estimates o f uncertainty derived from following this procedure are for in formation only, unless specifically instructed otherwise by the customer. The test conditions and limits defined in this part o f ISO 148 should not be adjusted to take account o f uncertainties o f measurement, unless specifically instructed otherwise by the customer. The estimated measurement uncertainties should not be combined with measured results to assess compliance to product specifications, unless specifically instructed otherwise by the customer. Instead, the indicated tolerances are to be interpreted as acceptance intervals. [5] This approach assumes that measurements are made with a tacitly accepted maximum measurement uncertainty. Where possible, this maximum measurement uncertainty has been specified in the current version o f the ISO 148 series. Measurement uncertainties of the measured values should be smaller than the indicated values. 22 © ISO 2016 – All rights reserved ISO 148-1:2016(E) E.3 General procedure E.3.1 Factors contributing to uncertainty T he pri ncip a l fac tors contributi ng to uncer ta i nty a re a s s o ci ate d with a) mach i ne bia s de duce d from the i nd i re c t veri fication, b) homo geneity o f the te s t materi a l and mach i ne rep e atabi l ity, a nd c) test temperature. T he me a s urement e quation for the me an ab s orb e d energ y KV is Formula (E.1): (E.1) KV = x − B V − Tx where x BV Tx i s the ob s er ved me an ab s orb e d energ y o f n te s t s p e ci men s; i s the i n s tru ment bi a s b a s e d on the i nd i re c t veri fic ation; is the bias due to temperature. E.3.2 Machine bias As a rule (see Reference [5 in ISO 148-2, as given in Formula (E.2): ] ) , me a s ure d va lue s s hou ld b e corre c te d for known bi a s . I nd i re c t veri fic ation i s one way to e s tabl i sh the va lue o f bi as . T he mach i ne bia s de term i ne d b y i nd i re c t veri fic ation i s defi ne d (E.2) B V = KV V − KVR where KVV KVR i s the me an va lue o f the re ference te s t pie ce s broken du ri ng the i nd i re c t veri fic ation; i s the cer ti fie d va lue o f the re ference te s t pie ce s . Depending on how well the value of BV is known, different actions are proposed in ISO 148-2 which de a l s with the u ncer tai nty a s s o ci ate d with the re s u lts o f i nd i re c t veri fic ation . a) BV is well known and stable. In this exceptional case, the observed value x equal to BV to obtain KV . f f f B V. In this case, the bias is not corrected for, but it contributes to uV f i s corre c te d b y a term b) M o s t o ten, there i s no fi rm evidence ab out the s tabi l ity o , the uncer ta i nty o I n b o th c a s e s , an u ncer ta i nty, the va lue o the i nd i re c t veri fic ation re s u lt. uV , as s o c iate d with the i nd i re c t veri fication re s u lt and the mach i ne bi a s i s ca lc u late d i n accorda nce with pro ce du re s de s crib e d i n I S O 14 8 -2 . T he outcome o f the uncer ta i nty ana lys i s o f the i nd i re c t veri fic ation i s the va lue uV. I f there i s a s igni fic a nt d i fference b e twe en the va lue s o f b e mu ltipl ie d b y the ratio © ISO 2016 – All rights reserved KV KV V . KV V and KV , then the values BV and uV should 23 ISO 148-1:2016(E) E.3.3 Machine repeatability and material heterogeneity The uncertainty o f x , the mean observed absorbed energy o f n test specimens, is determined using Formula (E.3): u (x) = sx n (E.3) where sx is the standard deviation of the values obtained on the n test samples. The value sx is caused by two factors: — machine repeatability; — sample-to-sample material heterogeneity. These factors are confounded, and therefore, are both included in this term. It is recommended to report the total measurement uncertainty with the value o f sx as a conservative measure for the variation in KV due to material heterogeneity. The value of ν x , the number of degrees of freedom of u( x ) , is calculated as n -1. E.3.4 Temperature bias The effect of temperature bias, Tx, on the absorbed energy is extremely material dependent. I f steel is tested in the brittle-to-ductile transition region, small changes in temperature can correspond to large di fferences in absorbed energy. At the time o f publication, it is not possible to present a generic and accepted approach to the calculation o f the contribution to absorbed energy uncertainty corresponding with the uncertainty o f the measured test temperature. Instead, it is proposed to complement the statement o f the measurement uncertainty in terms o f absorbed energy with a separate statement on u T, the uncertainty o f the test temperature at which the absorbed energy was measured (see E.5 for example). E.3.5 Machine resolution The effect of machine resolution is in most cases negligible in comparison with the other factors contributing to uncertainty (see E.3.1 to E.3.4). An exception is the case where machine resolution is large and the measured energy is low. In that case, the corresponding uncertainty contribution is calculated using Formula (E.4): u (r) = r 3 where r is the machine resolution. (E.4) The corresponding number o f degrees o f freedom is ∞. E.4 Combined and expanded uncertainty To calculate u ( KV ) , the factors contributing to uncertainty (see E.3) should be combined. Since u T is treated separately, and since the terms u( x ) , uV and u(r) are independent of each other, the combined standard uncertainty is determined using Formula (E.5): u( KV) = u 2 ( x ) + u V2 + u 2 ( r) (E.5) To calculate the expanded uncertainty, the combined standard uncertainty is multiplied by the appropriate coverage factor, k. The value of k depends on ν KV , the effective degrees of freedom of 24 © ISO 2016 – All rights reserved ISO 148-1:2016(E) ( ) u KV , which can be computed using the simple Welch-Satterthwaite[4] approximation, by combining the degrees of freedom, vV and vx, and evaluating the corresponding uncertainty contributions, uV and u ( x ) . Since the value of the degrees of freedom corresponding to u(r) is ∞, the machine resolution does not contribute to ν KV , see Formula (E.6): ν ( ) u 4 KV = KV u 4 x () νx + (E.6) uV4 νV NOTE In the case o f Charpy tests, the number o f samples is o ften limited to 5 or even 3. In addition, the heterogeneity o f the samples o ften leads to a significant value o f u x . This is why the number o f e ffective degrees o f freedom is most o ften not su fficiently large to use a coverage factor o f k equal to 2. () The coverage factor, k, corresponding to a confidence level of about 95 % is obtained from the GUM t-table as t 95 ν KV . (For selected t-values, see Table E.5 .) The expanded uncertainty o f KV is determined using Formula (E.7): ( ) ( ) ( ) ( ) ( ) (E.7) U KV = k × u KV = t 95 v KV × u KV E.5 Example In this example, the measurement uncertainty is calculated for the mean value, x , of a set of n = 3 samples from a particular test material. The results in Table E.2 were obtained on a pendulum which was success fully checked with both direct and indirect verification procedures. As a first step, the mean observed KV value, x , is calculated, as well as the standard uncertainty, u x , which is calculated using Formula (E.3). © ISO 2016 – All rights reserved () 25 ISO 148-1:2016(E) Table E.2 — Raw Charpy test results Dimensions in joules Test results KV, Sample 1 KV, Sample 2 KV, Sample 3 Mean KV, x 105,8 109,3 112,2 109,1 3,2 Standard deviation of n = 3 KV-values, sx S ta nd a rd u ncer ta i nty o f the me a n observed KV, u( x ) , calculated according to Formula (E.3) 1,9 In the second step, the raw results (without correction for bias) were combined with the results of the mo s t re cent i nd i re c t veri fic ation te s t, for wh ich re ference te s t pie ce s o f d i fferent energ y level s (e . g. 2 0 J , 1 2 0 J a nd 2 2 0 J ) were u s e d . T he te s t materi a l h ad a n ab s orb e d energ y level clo s e s t to the 1 2 0 J level (x = 10 9,1 J ) . T here fore, the i nd i re c t veri fic ation re s u lts ob tai ne d at th i s energ y level were u s e d i n the uncer ta i nty as s e s s ment. T he bia s va lue, BV , me t the veri fic ation criteri a i n accorda nce with I S O 14 8 -2 . BV, the measured value was not corrected for the bias. Therefore, the reported KV value, KV , is equal to the mean value, x , of the measured values. Since Si nce there i s no fi rm evidence ab out the s tabi l ity o f the me as u re d va lue was no t corre c te d veri fication re s u lt, uV for the bi a s , it contribute d to the uncer ta i nty o f the i nd i re c t . T he re s u lti ng s tand ard uncer ta i nty o f the i nd i re c t veri fic ation re s u lt at 1 2 0 J was uV = 5,2 J, with a number of degrees of freedom equal to 7 (see ISO 148-2). This information should be avai lable i n the i n s tr u ment do s s ier, wh ich i s up date d a fter e ach veri fic ation . Table E.3 give s the me a s u rement u ncer tai nty c a lc u lation pro ce du re . Table E.3 — Calculation scheme of expanded measurement uncertainty, U ( KV ) Raw test results R s u l t s f 1,9 J u (x) Degrees of freedom νx for tests on n = 3 samples, calculated as n −1 C o mb i ne d s ta nd a rd u ncer ta i nty ν e 2 r o m i n d i r e c t v e E xp a nde d u ncer ta i nty Table E.4 26 f i c a t i o n a D e gre e s o f fre e dom o f i nd i re c t ver i fic atio n νV, ta ken fro m c a l ib ration cer ti fic ate 8 a nd a 9 5 % con fidence level , t 1 2 0 J 5,2 J 7 5,5 J 8 KV , the effective degrees of freedom of u ( KV ) , from Formula (E.6) o i uV u ( KV ) , from Formula (E.5) t-factor corresponding with a ν KV f r 2,3 t 95 (ν KV ) 12,6 J U ( KV ) c a n b e u s e d to rep or t the te s t re s u lts a nd me as u rement u ncer tai nty. © ISO 2016 – All rights reserved ISO 148-1:2016(E) Table E.4 — Summary table of the result, KV , with expanded measurement uncertainty, U ( KV ) n sx a KV J a 3 This J 109,1 3,2 s ta nd a rd de vi atio n is a ν co n s er vati ve KV t 95 (ν KV ) 8 2,3 o f the e s ti m ate te s t m ater i a l U ( KV ) b, c J 12,6 he tero ge ne it y (i ts va lue also co nta i n s a co ntr ib utio n fro m the m ach i ne re p e atab i l i t y, wh ich c a n no t b e s ep a rate l y a s s e s s e d) . b c T he e xp ande d u ncer tai nty, calcu late d i n accordance with th i s pro ce dure, corre s p ond s to a con fidence level o f ab out 9 5 % . T he u nce r ta i nt y quo te d i s s ub j e c t to a n u nce r ta i nt y o f the te s t temp e ratu re , wh ich wa s me a s u re d to a n u ncer ta i nt y o f 2 K (co n fidence le ve l o f 9 5 %) . T he u nce r ta i ntie s quo te d do no t co n s ide r co ntr ib utio n s th at c a n b e i ntro duce d b y p a r tic u l a r characteristics of the test material. F i g u r e E . 1 — S t r u c t u r e o f t h e m e t r o l o g i c a l t r a c e a b i l i t y c h a i n f o r t h e d e f i n i t i o n a n d dissemination of the absorbed energy scales of the Charpy impact test © ISO 2016 – All rights reserved 27 ISO 148-1:2016(E) (v) from the t-distribution for v ff (v) +tp(v) that encompasses the fraction, p, of the distribution[5 ] Table E.5 — Value of tp an interval − tp to d Degrees of freedom, v 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 25 30 35 40 45 50 100 ∞ 28 tp e g r e e s o r e e d o m t h a t d e f i n e s (v) for fraction P = 95 % 12,71 4,30 3,18 2,78 2,57 2,45 2,36 2,31 2,26 2,23 2,20 2,18 2,16 2,14 2,13 2,12 2,11 2,10 2,09 2,09 2,06 2,04 2,03 2,02 2,01 2,01 1,98 1,96 © ISO 2016 – All rights reserved ISO 148-1:2016(E) Bibliography [1] [2] [3] [4] [5] [6] [7] [8] ISO 148-3:2016, Metallic materials — Charpy pendulum impact test — Part 3: Preparation and characterization ofCharpy V-notch test pieces for indirect verification ofpendulum impact machines ISO 3785, Metallic materials — Designation of test specimen axes in relation to product texture ISO 14556, Metallic materials — Charpy V-notch pendulum impact test — Instrumented test method ISO/IEC Guide 98-3:2008, Uncertainty of measurement — Part 3: Guide to the expression of uncertainty in measurement (GUM:1995) JCGM 106:2012, Evaluation ofmeasurement uncertainty — The role ofmeasurement uncertainty in con formity assessment ASTM E23, Standard Test Methods for Notched Bar Impact Testing of Metallic Materials LI H., ZHOU X., XU W Correlation Between Charpy Absorbed Energy Using 2 mm and 8 mm Strikers. J. ASTM Int. 2011 October, 8 (9) [JAI] NANSTAD R.K., SWAIN R.L, BERGGREN R.G Influence of thermal conditioning media on Charpy specimen test temperature. Charpy Impact Test: Factors and Variables, ASTM STP 1072. ASTM, 1990, pp. 195. © ISO 2016 – All rights reserved 29 ISO 1 48-1 : 2 01 6(E) I CS 7 7 . 0 40 . 1 0 Price based on 29 pages © ISO 2016 – All rights reserved
0
You can add this document to your study collection(s)
Sign in Available only to authorized usersYou can add this document to your saved list
Sign in Available only to authorized users(For complaints, use another form )