i An update to this article is included at the end Materials and Design 87 (2015) 1072–1086 Contents lists available at ScienceDirect Materials and Design journal homepage: www.elsevier.com/locate/jmad A review of ultrasonic peening treatment Massoud Malaki a,⁎, Hongtao Ding b a b Young Researchers and Elite Club, Islamic Azad University, Najafabad Branch, Najafabad, Iran Mechanical and Industrial Engineering Department, University of Iowa, Iowa City, IA 52242, USA a r t i c l e i n f o Article history: Received 10 July 2015 Received in revised form 18 August 2015 Accepted 20 August 2015 Available online 28 August 2015 Keywords: Ultrasonic peening treatment Peening Fatigue Stress concentration Residual stress Cold working Welding a b s t r a c t Ultrasonic peening treatment (UPT) has recently had significantly more attention in several manufacturing processes. UPT modifies the surface of a material and enhances the mechanical and/or chemical properties. This is especially true for welded components when working under fatigue dynamic loading conditions. The current review paper has been devoted to introduce this technology for its underlying mechanisms and effects. The UPT tools and devices are reviewed in terms of device configurations and process conditions. The effects of UPT are thoroughly discussed in terms of fatigue performance, resistance to wear and corrosion, and micro-structural evolutions. © 2015 Elsevier Ltd. All rights reserved. 1. Introduction Ultrasonic peening treatment (UPT) is one of the most promising methods in the cold treatment of metallic materials, particularly welded structures. This technique has many industrial applications such as aerospace [1], ship and marine [2–4], automotive [5], railway [6], and bridge structures [7], in which materials with very high strength, fatigue life, corrosion and wear resistance are needed. During the process, lowamplitude high-frequency ultrasonic oscillations are applied through a number of cylindrical rods or pins to the surface of metallic materials. Surface layers receive severe plastic deformation leading to the reduction of grain size, microstructural refinement, and geometrical modification. Superficial micro cracks are closed due to plastic deformation caused by the peening. Harmful tensile residual stresses are effectively eliminated [8] and a layer of compressive residual stresses is exerted to the metal surface. The UPT process is therefore able to increase surface micro-hardness, corrosion resistance, and enhances fatigue life and strength. UPT was firstly invented by Mukhanov and Golubev [9] in the 1950s. By generating continuous ultrasonic vibrations at a carburized steel tool tip, the treated part surface received direct impacts. In 1960, Krylov and Polischuk [10] proposed a spherical shot between a surface and ⁎ Corresponding author. E-mail addresses: massoudmalaki@aut.ac.ir, massoudmalaki@gmail.com (M. Malaki), hongtao-ding@uiowa.edu (H. Ding). http://dx.doi.org/10.1016/j.matdes.2015.08.102 0264-1275/© 2015 Elsevier Ltd. All rights reserved. ultrasonic transducer which imposed high plastic deformation. However, free motion of a spherical shot resulted in negative effects. Some comparative research works proved that cold hammer peening (approximately 5000 blows/min) is better than that of weld toe grinding [11–13]. Statnikov et al. [14] patented several inventions and significantly advanced different peening methods. They developed an ultrasonic magnetostrictive oscillating system with a peening tool and then applied the process to improve the quality and reliability of welded rail [15] and tubular structure [16] joints. Similar to hammer peening and needle peening, ultrasonic peening aims to redistribute residual stresses by eliminating tensile stresses, and introducing compressive stresses [17–21]. The main difference of the peening methods mentioned above and the UPT is in the vibration frequency of their peening tools. Both needle peening and hammer peening methods are pneumatic actuated systems with a vibration frequency of 50–1000 Hz, while the common operational frequencies are much higher at 20 kHz or more for the UPT process. This range of frequency makes UPT a quiet material processing method. In hammering and needling, the exerted force on the treated surface is of vital importance, and often is greater than 20 kgf. Due to intensive impacts, high amounts of noise and vibrations are transmitted to the operator's hands, making it hard to keep the peening tool at a correct angle and direction. Treatment duration in the UPT process is usually much shorter because of high frequency mechanical impacts. Compared with hammering and needling, UPT is comfortable and effective with much lower noise [22,23]. In addition, workpiece material responds differently and material softening often occurs while processing in the ultrasonic frequency domain [24]. M. Malaki, H. Ding / Materials and Design 87 (2015) 1072–1086 1073 Fig. 3. Different designs with changeable UPT working heads: (a) one four-pins working head with the pin diameter of 3 mm; (b) one three-pins working head with the pin diameter of 4 mm; (c) one seven-pins working head with the pin diameter of 5 mm; (d) one single-pin working head with the pin diameter of 4 mm [33]. Fig. 1. Ultrasonic peening gun and system (courtesy of SINTES Company). UPT and the other peening methods such as needle peening treatment, high-frequency mechanical impact treatment, and hammer peening, are all cold mechanical treatment methods in which a dense, compressed layer of material is produced on the component surface. In these methods, a number of vibrating pins or rods are commonly implemented for impacting material surface. Other peening techniques have been developed using different forms of tools, which may not be a cold working process. For instance, shot peening (SP), laser shock peening (LSP), and cavitation peening (CP) are widely used. Being similar to sandblasting, shot peening process is a cold-based treating method for modifying material surface upon which surface micro-cracks or tensile residual stresses exist. SP is commonly used for aircraft repair, gear parts, turbine components, connecting rods, etc. [25]. During SP, specimen surface is bombarded by small spherical shots in a randomly impacting fashion. The thickness and material behavior of the treated layer is not homogenous throughout the surface under this treatment. Thin work pieces and sharp edges are subject to Fig. 2. Ultrasonic peening tool invented and fabricated by Prokopenko et al. [37]. deformations in the shot peening process. In the LSP treatment, the surface is treated with a high energy laser beam with a pulse of energy of several Joules during a few nanoseconds. A shock wave is generated due to the volume expansion of the plasma plume forming on the surface and propagating into the material substrate [26]. Although LSP process has a deeper treatment depth than TIG dressing, the process is more expensive, often too slow to scan a large area, and rather difficult in controlling its process parameters. In addition, it requires advanced installation and clean environment for the operation. As a newly developed technique in practical industries, CP is a peening process utilizing high pressure impacts induced by the collapse of ultrasonic cavitation bubbles near the materials surface in liquids [27, 28]. Generation of shock waves leading to liquid microjet development is the main principal of the cavitation peening. This process is very sensitive to the process parameters, and an improper design of the process variables may cause irreparable side effects [29]. Compared with the other techniques, ultrasonic peening process has a number of benefits including high productivity, low cost, better mobility with light weight components, and good flexibility of working on different types of welds in various attitudes and cleanliness. The UPT process can be applied in both manufacturing and repairing stages for small treating areas. In this paper, the technical advancements and research works on the UPT will be thoroughly reviewed. In Section 2, the design of UPT tools and devices will be discussed in terms of device configurations, elements, process parameters, etc. In Section 3, the underlying process mechanisms and theoretical hypotheses are presented. In Sections 4 and 5, the effects of UPT on the fatigue performance, hardness, corrosion, and microstructural evolutions will be reviewed and discussed. Section 6 is devoted to reviewing the existing numerical studies. Fig. 4. Impact heads used for the UIP processing of flat (a, c) and round-bar (b) samples [38]. 1074 M. Malaki, H. Ding / Materials and Design 87 (2015) 1072–1086 Fig. 5. (a) Geometrical modification in the weld toe region by UPT in order to reduce/remove weld toe convex areas and produce a smoother transition from the weld to the parent base metal [51]. (b): The view of butt weld in as-welded condition. (c): The view of butt weld treated by UPT [33]. 2. Design principles for UPT devices The ultrasonic peening treatment method is based on both the effect of high frequency low amplitude impacts of a power ultrasonic hammer Fig. 6. (a): Notch existence in the weld toe of specimen without peening; (b) Closed cracks in the weld toe of specimen treated by UPT [30]. gun, and the vibrations in the material under the treatment. Fig. 1 shows a simple configuration of ultrasonic peening system. An ultrasonic peening gun commonly includes the power supply of hundreds to thousands of watts generating electrical current with specific power, frequency and voltage. A magnetostrictive or piezoelectric sandwich transducer is used to convert input electricity received from the power supply to high frequency oscillations. The system has an optional concentrator or transmitter to deliver vibrational energy from the transducer to the tool tip(s). A computer kit controls and optimizes the energy delivered to the workpiece and can also keep the vibrating tool in a resonance condition. Most of the time, a cooling system is used as the transducer gets hot after a long operating period of time. The vibrating transducer can be either magnetostrictive or piezoelectric. The piezoelectric type of ultrasonic peening is newer than the magnetostrictive type, outperforms the magnetostrictive type, has lighter components, and is easier to use and move. A pumped cooling water system is mandatory for the magnetostrictive type due to heat generation and energy loss in the transducer, which increases the equipment cost and makes the system more complicated and heavier. Compared with the magnetostrictive-transducers containing the aforementioned drawbacks, the piezoelectric types are often selected. Piezoelectric type of ultrasonic peening tools commonly have the working frequencies of 20–55 kHz [30,31], vibration amplitudes of 20–50 μm [32,33] and powers of 300 W–4 kW depending on the aim of the treatment [33–35]. A typical piezoelectric type of ultrasonic peening tool is illustrated in Fig. 2. It receives a high voltage, high frequency electrical current from the power supply (1). A pair of piezoelectric materials (3) is tightened between the two mechanical elements of backing part (2) and matching part (5), between which electrode(s) (4) are arranged. A mechanical concentrator (6) operatively attached to the matching part concentrates vibrational energy and then delivers it to the next part. At the end part of the tool, a holder (7) for a flat shaped spring, (8) and an elastomeric retaining element (9) have also been provided. Made of high strength steel, the steel plate (10) is connected to the free end of the rod pins. Rod shaped tools/pins with the rounded ends (11) are joined to the end point of M. Malaki, H. Ding / Materials and Design 87 (2015) 1072–1086 1075 Fig. 7. TEM observations of the grain structure in the top surface layer (on the depth of about 10 mm) of metallic materials after the UPT with simultaneous shifting of sample for 4 min: (a, b) AISI 321 stainless steel, (c, d) VT1-0 titanium alloy, (e, f) VT6 titanium alloy and (g, h) LCB titanium alloy; (a, c, e, g) bright field images and (b, d, f, h) dark field images [38]. the tool. These pins deliver ultrasonic vibration to the workpiece (12). The projection part (13) helps by using passive cooling. The elastomeric casing (14) filled with a suitable liquid (15) is attached to the concentrator. The liquid functions as both coolant and lubricant. Depending on different conditions, different numbers of pins with different arrangements can be used. Fig. 3 shows some different tool tips/pins. Also, it has already been accepted and established that intense, effective and efficient plastic deformation of the material surfaces can only be achieved if the rod tool tips (strikers) are not rigidly connected to the concentrator [36]. The pins or rods should freely vibrate between the vibrating transducer and workpiece. Mordyuk et al. suggested a combination of both vertical and lateral impacts and developed a sliding peening impact process [38]. As shown in Fig. 4, the lateral load component is added to the peening process. With simultaneous vertical and lateral load components, their research showed that higher evenness of the surface structural state could be achieved. The UPT process can create a homogenous, fine and smooth surface, which is not only faster but also easier to control than other peening methods such as shot peening. It should be noticed that the lateral vibration of the tool or specimen for creating sliding impact may lead to a decrease in the surface micro-hardness or even the thickness of nano-crystalline layer induced by the deformation. To design, simulate and manufacture the UPT devices, mathematical approaches [39] and numerical modeling methods such as finite element simulations [40,41] are often applied. The main part of any UPT device is its actuator part consisting of backing part, piezoelectric ring(s) and matching part. Tightened by a steel bolt between the two backing and matching parts, piezoelectric rings receive and convert electrical energy into mechanical vibrations. The matching part is often made of aluminum or titanium alloys, while the backing is usually 1076 M. Malaki, H. Ding / Materials and Design 87 (2015) 1072–1086 Fig. 8. Weld toe micro hardness values and distributions: with the UPT (1 and 2), without the UPT (4, 5), without the UPT and with the fatigue test (7, 10, and 11), with the UPT and the fatigue test (13, 16 and 17). made of a heavy, dense material such as steel alloys. The ultrasonic waves are delivered from the piezoelectric rings to the concentrator through the active resonant surface of the matching part, and the backing part prevents acoustic energy loss in the other free end. Further information can be found in the literature, for example see Refs. [42,43]. The actuator part should vibrate with the fundamental resonant frequency to avoid mechanical or heat losses. Therefore, the length of it should be equal to half of wave length. Furthermore, the total length of the UPT device should also be a multiple of wavelength. Both modal and harmonic simulations are available in the FEM software programs like ANSYS and ABAQUS, two of the most prevalent computer programs in the design and simulation of ultrasonic devices. For fabricating the UPT components, materials must be selected from high strength metals for enduring life under static and dynamic loading conditions. Light aluminum alloys with the lowest vibration damping are commonly selected for the fabrication of matching and concentrator parts of UPT [44]. Also, surface finish of these components should be as high as possible to prevent wave propagation and dispersion. Materials used for the pins must be from hardened high-strength steels resistant against wear, corrosion, and brittle fracture. MPIUltrasonics, and Applied Ultrasonics are of worldwide well-known manufacturers of different ultrasonic transducers which are used in different applications like UPT devices. Fig. 9. Polarization curves taken from 1: base metal of St 304, 2: weld toe of peened specimen, 4 and 5: weld toe of as-welded specimens in NaCl3.5% solution of the potentiostat system [30]. 3. Underlying mechanisms Geometrical modification is often achieved by the UPT for the weld toe region to reduce/remove weld toe convex areas and produce a smoother geometrical transition from the weld to the parent base metal [50]. As demonstrated in Fig. 5, UPT produces a layer of favorable compressive residual stresses in the weld toe region, and decreases the concentration of external stresses and tensile residual stresses in the welded elements. As a result, a smoother transition from the welded joint to the parent metal occurs by formation of a groove in the melting zone of the welded joint with the base metal [31,45,46]. With the acoustic softening (or acoustic plasticity) effect, the UPT acoustic irradiation field can decrease the value of stresses needed for the plastic deformation. The phenomenon, which takes place promptly when a material is subjected to ultrasonic vibrations, has already been observed and established in several metallic materials, like stainless steel and titanium, in different technological/manufacturing processes [8,47–50]. Surface state has an important effect on material failure including fatigue failure, corrosion failure and wear failure [52]. Without changing the slope of S–N curve, UPT has been found to be able to improve the weld toe geometrical profile [32,53,54], modify the surface residual stresses with more compressive stresses, eliminate or reduce distortions caused by welding or other technological processes [33], and change the microstructure of the welded parts by exerting a layer of cold worked high plastic deformations at the weld toe region [55,56]. Modification of surface residual stress has been extensively studied for the UPT process. For instance, Cheng et al. [57] conducted an experimental research on post-weld treatment and analyzed its beneficial effect on the fatigue strength of welded structures. To measure the residual stress modification, X-ray and neutron diffraction measurements were performed on specimens produced by ultrasonic peening of A572 Gr.50 steel. These measurement results showed that compressive residual stresses were induced on a surface layer of 1.5–1.7 mm in depth and ± 15 mm in width. The peak compressive stresses of −427 MPa, and −458 ± 20 MPa were found in the parallel and perpendicular directions to the treatment line, respectively, both of which exceeded the nominal compressive yield stress. Janosch et al. [58] conducted a similar experimental study for residual stress analysis before and after the UPT using hole drilling stress measurement method. Compressive residual stresses close to the nominal yield stress was determined in the region under the UPT treatment [58]. The microstructural features including nanograins, microbands, high-density M. Malaki, H. Ding / Materials and Design 87 (2015) 1072–1086 1077 Table 1 Corrosion parameters of the AISI-321 samples studied in a 3.5% NaCl solution. Sample Ecorr (mV) vs. SCE lg(icorr) (A cm−2) lg(ip) (A cm−2) Ebd (mV) References AISI-321, as-annealed AISI-321, after UP; 1 min AISI-321, after UP; 2 min AISI-321, after UP; 3 min AISI-321, after UP; 4 min 1Cr18Ni10Ti, as-received 1Cr18Ni10Ti, shot-peened AISI-304SS, as-received AISI-304SS, sandblasted AISI-304SS, sandblasted + annealed −384 −298 −281 −253 −474 −330 −375 −250 −370 −260 −6.68 −7.03 −6.91 −6.89 −6.74 −7.4 −9.2 −8.2 −7.7 −8.2 −5.41 −5.82 −5.51 −5.67 −5.83 – −6.4 −6.3 −5.5 −6.2 – +289 +198 +193 – – +350 +90 −60 +100 [35] [35] [35] [35] [35] [71] [71] [72] [72] [72] dislocation, and twining structure can be induced to the surface material by UPT [59–62]. Using the high plastic deformation of the UPT, this process is able to effectively change grain shape and size to about 10 nm [63]. As shown in Fig. 6, surface and subsurface micro cracks, cavities and voids can be effectively closed by the UPT, which helps elevate the fatigue endurance limit and crack growth threshold. Weich et al. [64] studied the crack nucleation and propagation for the welded structures of two high strength steel materials (steel grade S355J2 and steel grade S690QL) treated by high frequency mechanical impacts. In as-welded butt joints, small cracks were initiated in many positions. They then propagated parallel to one another and finally connected with each other in order to create an elliptical crack. On the other hand, microcracks were caught in a depth of about 2 mm for the treated materials and only one single crack could initiate and grow, finally leading to the fracture. It was also proved that crack propagation rate was much slower in the treated specimens than that of as-welded conditions. 4. Metallurgical effects In this section, the UPT different effects on the micro-structures and metallurgical properties are presented. Generation of a nanocrystalline layer, corrosion resistance improvement, and hardness increase are key effects of the UPT on the metals, steel materials in particular. 4.1. Nano-crystalline structure A surface layer of nanocrystalline microstructure could be produced by implementing the UPT due to the effect of severe plastic deformation exerted on the topmost surface layer. A number of investigations have shown that a nanocrystalline layer of 30–50 μm in thickness can be achieved by the UPT as can be seen in the research work by Mordyuk and co-workers [35,61], Roland et al. [62] and Darling et al. [65]. The nanocrystalline layer formation strongly depends on the material properties and the UPT operational parameters such as the duration of the process [63]. Mordyuk and Prokopenko [38] studied surface properties produced by the UPT and reported surface grain refinement at the top superficial layers of ultrasonic peened specimens. This layer of hard material makes it more resilient against corrosion and wear [66]. TEM micrograph showed an average grain size of 10–100 nm in an ultrasonic peened specimen consisting of stress induced austenitic martensite. Fig. 7 shows the deformation-induced martensite. The same ultrasonic peening condition led to formation of a nano-grain size of up to 10 nm in α titanium alloy (VT1-0), and 20–100 nm for α + β titanium alloy (VT6). increases dislocation motion and the density of material defects and dislocations increase. Under ultrasonic peening action, the grain crushing, refining and reforming are expected. As a result, surface hardness and corrosion resistance increase. Fig. 8 shows the micro hardness values before and after the UPT, plus before and after fatigue tests [30]. Regarding the corrosion resistance of the UPT treated materials, many research works have been done and state UPT results in superior metallurgical properties [68–70]. The grain boundaries are first corroded when the surface of the material is exposed to a corrosive chemical, since grain boundaries have a high level of energy and are chemically active. Both the HAZ and the weld material are not resilient against inter-granular corrosion, stress corrosion cracking, and pitting/crevice corrosion. By applying UPT, a deformed layer of dense compressed material is generated in the weld toe region which is resilient against corrosive solutions [52]. Under this circumstance, the interaction between the grain boundaries and corrosive materials will be minimal. Abdullah et al. [30] performed an experimental analysis on the UPT and found a 100% improvement in corrosion resistance for the ultrasonically peened specimens of St-304 welded parts. As shown in Fig. 9, the values of mean electrical resistance were 1.8 × 10+6 Ω and 6.6 × 10+6 Ω respectively for as-welded and ultrasonically peened St-304 welded joints. Furthermore, the values of corrosion rate were measured as 0.022 mm/yr and 0.0044 mm/yr respectively for as welded and ultrasonically peened specimens. Other studies have also paid attention to the corrosion resistances of different stainless steel materials having a nanostructured surface induced by severe plastic deformation processes [30,71,72]. The logarithm of corrosion current density against electrical potential is shown in this figure. The corrosion current density (Icorr) 4.2. Corrosion resistance and hardness UPT is frequently reported to have a significant effect on both wear and hardness values. It was validated that both nano-scale structure and compressive residual stress contribute to the hardness and wear increase [67]. When the UPT process is applied, plastic deformation Fig. 10. Effectiveness of different fatigue life enduring post-processing techniques of SSAB Weldox 420 welded joints (1) as-welded condition, (2) UPT by a 5 mm diameter multi-pin tool, (3) treated by hammering, (4) shot peening, (5) TIG dressing, (6) TIG dressing and UPT, (7) UPT by a 3 mm diameter multi-pin tool [86]. 1078 M. Malaki, H. Ding / Materials and Design 87 (2015) 1072–1086 Fig. 12. Fatigue behavior of low carbon steel welds. (1) as-welded, (2) after UPT, immediately after welding process, (3) after the UPT, after prior cycling up to 50% of the fatigue life of as-welded joint [38]. Fig. 11. Weld toe UPT treated; (a) Under-treated weld toe (reduced intensity); (b) Under-treated weld toe (increased speed); (c) Over-treated weld toe; (d) Properly treated weld toe (robotically); (e) Properly treated weld toe (manually) [93]. and corrosion potential (Ecorr) of each specimen can be determined through the polarization curves. Based on Faraday's law and graphical analysis of polarization results, higher corrosion potential is equivalent to higher corrosion resistance and vice versa. Table 1 summarizes the corrosion behavior of steel materials treated by different techniques. It was found that shot peening deteriorates corrosion resistance but the UPT enhances it [73]. The corrosion current density (icorr) is calculated considering the cathodic and anodic Tafel curves and their slopes. ip is the passivation-maintaining current density. The breakdown potential (Ebd) is the potential at which the anodic current significantly increases. Similar work showed that the corrosion resistance was deteriorated after the shot peening treatment for 12% Cr steel specimens. The difference in corrosion performance by SP and UPT can be attributed to the surface quality after the treatment. The surface roughness created by the UPT is better than the one by the SP because increasing surface roughness leads to the increase of the practical area for corrosion per unit area [74]. Mordyuk and Prokopenko [75,76] analyzed the effect of surface roughness on corrosion and found that micro coarseness or cracks is a vital issue, which induces stress concentration and facilitates the surface crack initiation under dynamic loading conditions. As a result, the UPT process should be carefully designed and managed. It is critical to choose proper processing parameters that the resultant surface roughness can be minimized for substantial benefits [38]. For the sliding peening impact process, they proposed a combination of both vertical and lateral impacts. In this case, the lateral load component was added to the process (Fig. 4). With simultaneous vertical and lateral load components, better evenness was achieved. The effect of the UPT on the corrosion behavior still needs further investigations as it seems several parameters like peening method, micro-structural characteristics, galvanic effect, mechanical properties and chemical composition, temperature, etc. play important roles in the corrosion behavior. For instance, Barbucci et al. [77] found that the strain induced martensite has a negative, detrimental effect on the corrosion behavior of cold rolled AISI 301 stainless steel. However, Lee et al. [73] showed that it has a positive effect on the corrosion behavior of the UPT treated AISI 304 stainless steels. Mordyuk et al. [35], carried out the X-ray, TEM, and magnetic tests for the treated specimens by the UPT, showed the effectiveness of the UPT in enhancing corrosion resistance, and found that the peening process was accompanied by a strain induced martensitic transformation. In addition, hardness increase was found to be dependent on the grain refinement, strain-induced martensitic transformation, and the grain boundary dynamics. They also drew to attention that the more the volume fraction of strain induced martensite, the greater the probability of producing galvanic effects between austenite and martensite phases. 5. Mechanical effects In this section, mechanical effects are discussed. The UPT enhances mechanical strength through closing cracks, voids, and cavities. The UPT mechanical effects vary in degree and amount depending on what kind of materials, welding process, and treatment conditions are implemented. 5.1. Fatigue improvement The most important effect with the UPT is its effect on fatigue. Extensive research efforts have been focused on the UPT fatigue enhancement and the involved parameters. In 1970, Statnikov firstly used ultrasonic impact peens in separate holes on the vibrating head for working on welded and machined parts, and exerted high plastic deformation on the material surface. Appearing to be less affected by corrosion than TIG dressing and re-melting methods, Kirkhope et al. [2] concluded that hammer peening gave the greatest improvement in corrosion fatigue behavior of ship structures than that of TIG or burr grinding processes. In addition, the fatigue strength improvement of hammer M. Malaki, H. Ding / Materials and Design 87 (2015) 1072–1086 1079 Table 2 The fatigue strength of as-welded and treated joints under constant amplitude (CA) and variable amplitude (VA) loading conditions [94]. Treatment Loading condition Fatigue strength (2 × 106) Δσ (MPa) Improvement (%) Loading condition Fatigue strength (2 × 106) Δσ (MPa) Improvement (%) UPT TIG As-weld CA CA CA 212 158 115 184 137 100 VA VA VA 198 147 110 180 134 100 peened specimens was reported to be twice as effective as specimens treated by TIG and grinding methods. Haagensen et al. [78,79] reported that increases in fatigue strength at 2 million cycles ranged from a negative effect for hammer peening of 6 mm aluminum lap welded plates to approximately 135% improvement for high strength steel specimens post-processed by the combination of the TIG dressing and the UPT method. Roy et al. [32] performed an experimental analysis on ultrasonic peening and found that fatigue strength of critical welded parts could be enhanced at least two AASHTO categories and as much as an 8 times improvement in fatigue life. Trufiakov et al. [80] performed the efficiency analysis of UPT on fatigue strength of welded joints and found that ultrasonic peening could improve the fatigue strength from 178 MPa to 351 MPa at the 2 million cycles TMCP steel. Nonetheless, a few contradictory results have also been reported. For instance, in a study carried on 2024-T3 aluminum welded details, it was shown that UPT drastically reduced fatigue life but enhanced superficial micro-hardness and exerted compressive residual stress [81]. Further studies are being done on light weight structures such as aluminum or titanium structures. UPT was shown as an effective method for treating welded steel structures under dynamic loadings with variable amplitudes [82,83]. Under dynamic loading conditions, decreasing the stress concentration coefficient in the transition area from the weld metal to the parent metal is of crucial importance [53,84,85]. For welded connections having high reactive residual stresses equilibrated within the volume of the structure, UPT could also enhance the fatigue lives by 50% more than the as-welded S355 J0 steel specimens of large structures [22]. Statnikov et al. [86] carried out a comparative study on treatment methods for transverse fillet welded specimens fabricated from structural steel (SSAB Weldox 420) by shot peening, TIG dressing, and UPT (using 3 and 5 mm diameter multi-pin tools). Their experimental analysis on fatigue performance showed that under correct and proper conditions, UPT produced the highest improvement in fatigue life as is shown in Fig. 10. The improvements due to hammering, TIG dressing, shot peening, and a combination of TIG dressing and UPT were found to be virtually the same increasing the fatigue life by 41–51% at 2 million cycles. In comparison, a 65–75% fatigue life enhancement was found in the specimens prepared by UPT. Fatigue life of high strength steels was shown to be much better enhanced by UPT than Low Transformation Temperature Electrodes (LTTE) [87,88]. According to the research work by Lixing et al. [88], fatigue strength improvement of steel specimens with transverse butt welded joints and longitudinal fillet welded gussets was respectively 50% and 71% at 2 million cycles after processing by ultrasonic peening action. However, the improvement was respectively 11% and 41% in each case of treatment by LTTE method. 5.2. Rehabilitation and maintenance UPT can be used in order to rehabilitate and repair welded structures e.g. flange gusset specimens in both original and repair conditions by an amount which approximately is equal to a 3-class raise in the JSSC procedures [45,89,90]. The UPT has been defined as an effective method in rehabilitating, repairing, and preventing fatigue crack initiation in the welded structures that are in service [6,38,45]. A similar enhancement can be achieved in fatigue strength and life for welded structures by UPT either during or after the manufacture [91]. Statnikov et al. [51,92] reported ultrasonic peening was the most effective method for large plastic deformations and fatigue strength improvement, which can be used before, during, and after the manufacturing process or even for maintenance and repairing welded joints. Also, not more than 4 treating passes was suggested by Statnikov et al. [31] to obtain the desired treatment. Further passes were not suggested because of not having sensible improvements [18]. Fig. 11 shows weld toe experiments of under-treated, proper, and over-treated specimens. The figure shows that the over treating process can also be destructive. As shown in Fig. 12, UPT was applied on carbon steel in two different cases: immediately after the welding process and after prior cycling up to 50% of the fatigue life of as-welded specimen. The improvement of curve 3 might be due to the relaxation of tensile residual stresses when preliminary cycling conditions. 5.3. Loading conditions This section discusses the effect of loading conditions with UPT and also other peening techniques. As shown in Table 2, under variableamplitude loading condition, Huo et al. in 2005 [94] studied the 16Mn welded steel joints (8 mm thick plates with longitudinal fillet welded attachments) in all the as-welded, UPT treated, and TIG dressed conditions. In both constant and variable amplitude loading conditions, both UPT and TIG dressing methods increased fatigue strength and life significantly. UPT could be even better than TIG. For the constant amplitude loading conditions, UPT could increase the fatigue strength and life by up to 84% and 3.5–27 times, respectively; for the non-constant amplitude loading conditions, UPT could increase the fatigue strength and life by up to 80% and 2.5–17 times, respectively. Mordyuk et al. [95] showed the UPT outperformed laser shock peening (LSP) of AISI 321 in several attributes. For instance, no change in phase composition occurred in the laser-peened parts. However, strain-induced martensite transformation was found to have occurred in the ultrasonically peened specimens. The thickness of surface compressive layer was almost 10 times higher in ultrasonically peened Fig. 13. Weld toe geometrical modification by different post-weld treatment methods; AW: as-welded, BG: burr grinding, TIG: TIG dressing, UPT: ultrasonic peening treatment [99]. 1080 M. Malaki, H. Ding / Materials and Design 87 (2015) 1072–1086 Table 3 Fatigue life prediction of UPT IS-2062 grade B carbon steel treated welded specimens through different standards [98]. Stress, MPa 250 300 350 Predicted fatigue life in cycles Experimental value in cycles BS 7608 (95% pos) BS 7608 (50% pos) BS 7608 (5% pos) AWS D1.1 97,248 56,278 35,440 255,200 147,685 93,003 669,699 387,558 244,060 92,646 53,614 33,763 IIW XIII-1539 128,000 74,074 46,647 Peened Unpeened Set I Set II Set I Set II 250,880 107,786 35,407 208,164 100,538 30,568 152,547 116,778 74,568 188,803 141,086 73,625 pos: probability of survival. specimens than that of laser peened specimens. Also, the micro hardness of ultrasonic peened parts was revealed 40% higher than that of laser peened materials. Since the compressive layer induced by the UPT was thicker and harder, a higher fatigue life and higher corrosion resistance could be expected for the UPT treated materials [96]. The effectiveness of UPT in lower applied stresses has been revealed in several studies. However, at the higher level of applied stresses, particularly those stresses which are close to the material yield stress, the UPT may not be effective with apparent improvement [97]. According to Jinu et al. [98], Pedersen et al. [99], and Zhuang and Halford [100], the main reason for the phenomenon mentioned above has been attributed to the relaxation of the compressive residual stresses exerted by the UPT. Of course, the UPT still has improvements due to weld toe geometrical modification. Fig. 13 shows the weld toe micrographs treated by all as-welded, burr grinding, TIG dressing, and UPT methods. Although the TIG method has created a smoother weld toe profile, the welding speed and the torch angle variations might be a serious problem since the process is rather complex and improper treatment can cause side effects. Through comparison of different fatigue test standards such as BS 7608 [101], AWS-D-1.1 [102] and IIW-XIII-1539-96 [103], with the experimental observations of the peened and non-peened IS-2062 grade B carbon steel, they found BS 7608 with 50% probability of survival is in the best agreement with the experiments. Table 3 shows their experimental results along with BS 7608, AWS D 1.1, and IIW-XIII-1539-96, and their calculated fatigue lives. In 2009, a comparison between shot-peening and ultrasonic peening was done by Lee and co-workers [73]. According to their results, ultrasonically peened parts showed an equal or better resistance in corrosive environments. Ting Wang et al. [104] studied three types of low, medium, and high strength steels, i.e. Q235B, 16Mn and SS800, for determining fatigue design differences between as-welded and UPT treated welded joints. They showed fatigue strength of UPT treated joints is dependent on average stress and UPT treated joints' S–N curves are much flatter so that m = 9 can be recommended for fatigue design of ultrasonic peening of weld joints. In this work, stress ratio and its effects on the fatigue life have also been proposed and discussed. A number of fracture initiation and growth mechanisms have already been introduced, analyzed, and discussed [105–110]. In 2010, Yin et al. [7] studied the fracture mechanisms of both as-weld and UPT treated welded joints made of high strength bridge structure steels, Q235B and Q345. For the as-welded state, a fatigue crack is initiated in the material surface because of the surface slag inclusions or second phase particles. However, a micro-crack in the peened compressive area was also observed which was generated by the ultrasonic peening energy. Of course, because of the mentioned layer, crack propagation rate is much lower in the UPT treated parts than that of as-welded joints. They concluded that the slope of S–N curve (m) should be set as 3 for the fatigue cycles less than 10 million and 5 for more than 10 million. It has to be set as 10 when treated by the UPT method [111]. Later, Zhao et al. [97] studied fatigue behavior of welded joints through S–N curves. A significant fatigue life and strength was seen for the UPT treated specimens in lower stress ranges (R = 0). For example, for a stress of 276 MPa, 105 and 2.3 × 106 cycles were reported as the fatigue life of as-welded and UPT treated specimens respectively. The fatigue life, therefore, was prolonged by 22–45 times for the tubular welded elements of 20 steel (R = 0). On the other hand, the UPT improvement was not apparent under high applied stress ratio (R = 0.5) [112]. According to Fig. 14, the slope of S–N curve for the UPT treated before loading (m = 5) is almost the same as as-received specimens Fig. 14. S–N curves for as-welded, UPT treated before loading and UPT treated during loading tubular 20 steel welded joints [97]. Fig. 15. The effect of UPT treatment on the fatigue strength with and without pre-load conditions [115]. M. Malaki, H. Ding / Materials and Design 87 (2015) 1072–1086 Fig. 16. UPT treated welded joints under different stress ratios [115]. (m = 3) in high stress ratios of R = 0.5. However, the UPT during loading was found to be much more effective than that of the UPT before loading as the fatigue life of the UPT treated specimens during loading was prolonged by 4.8–6 times. The differences between before loading and under loading UPT treatment cannot be attributed to either the microstructural feature caused by severe plastic deformation or internal stresses. It was claimed that the main reason of such a difference relies greatly on the surface layer stresses caused by the UPT in high stress ratio [113]. During loading in high levels of stress ratio, the UPT process induced compressive residual stresses and higher yield stress, and therefore better mechanical strength is obtained [97]. In 2011, another research on the fatigue properties of ultrasonically peened friction stir welded parts was performed by Yang et al. [114]. In this research, under stress ratio R = 0.5, fatigue life of welded joints of Al7075-T651 was prolonged by 8 ~ 14 times. Okawa et al. [115] investigated the effect of pre-load and different stress ratios on the fatigue strength of the UPT treated AH36 shipbuilding high-strength steel. In their study, pre-load stress tests were 1081 performed for tensile stress of 90% of the yield stress and compressive stress of 60% of the yield stress. They found that after the pre-load condition, the fatigue strength of the UPT treated welded joints slightly decreased. Fig. 15 shows the S–N curves of the transverse non-load carrying fillet welded joints subjected to the UPT or toe grinding with or without pre-load. As shown in the figure, the tensile and compressive pre-load had the similar effect. Furthermore, under several stress ratio conditions, the UPT was found effective in improving fatigue strength even at the R = 0.5 stress ratio as shown in Fig. 16. By applying UPT, fatigue strength improvement decreases as the stress ratios become higher [3]. The UPT fatigue strength improvement was examined on the welded elements with different thicknesses. Through different thickness plates (16, 22, 30 mm), Mori et al. [3] applied the UPT on several joint type parts commonly used in the construction of ship structures. They studied the role of load history and excessive tensile and compressive loading conditions on the fatigue strength improvement via UPT. They found that the UPT has an improving effect regardless of elements thickness. UPT fatigue strength improvement diminishes as the welded elements are exposed to excessive compression loading and is maintained when exposed to excessive tensile loading conditions as shown in Fig. 17. The best occasion for carrying out the UPT is after loading since it avoids losing the UPT effect because of the changing of the stress distribution [3]. As shown in Fig. 17, two cases were studied for UPT before loading (Case A) and after loading (Case B). In Case A, the weld toe is peened, excessive tensile stress is applied to the specimens as a mean stress, and a fatigue test is done. In Case B, however, excessive compressive stress is applied first, then the weld toe is peened and finally a fatigue test is done. It was revealed that the surface hardness of the peened aluminum metal matrix composite could be about 1.1 GPa even after the heat treatment to 623 K [116]. The first technical guide defining UPT parameters, criteria, and variations was firstly documented by Statnikov in 1999 [51]. Marquis et al. proposed detailed fatigue assessment guidelines for treating steel structures by high-frequency mechanical impacts [117]. For slightly exfoliated 7075-T6511 aluminum specimens used in aircraft upper wing skin panels, UPT could change the crack nucleation mechanism from the inter-granular to the fretting mechanism which means prolonged fatigue life [118]. However, for the severely exfoliated aluminum materials the cracks were nucleated from inter-granular cracking and no sensible fatigue life improvement was seen. 6. Numerical analyses The UPT process has rarely been studied numerically in the past, which was mainly due to complex material behaviors and a lack of Fig. 17. UPT effects on the fatigue life improvement of the ship elements before and after launching [3]. 1082 M. Malaki, H. Ding / Materials and Design 87 (2015) 1072–1086 Fig. 19. Comparison between the numerically obtained S–N curves and the results obtained by the experiments [113]. Fig. 18. ACPD (alternating current potential drop) crack growth measurement results. (a) Constant amplitude (CA) loading at ΔS = 270 MPa, R = 0.1. (b) ps-m-40 loading. (c) ps-r-15 loading. understanding of the process physics. On the other hand, experimental testing or measurements involve too many expenses. So in order to reduce the cost and time spent on studying the different effects UPT has on the mechanical or chemical properties, it is essential to pay more attention to this field of study, i.e. developing computer models in order to obtain the most reliable and accurate results as possible [18,20,119–121]. Using Chaboche kinematic hardening material model used in ABAQUS/Explicit, Baptista et al. [20] produced a dynamic simulation code for the hammer peening of T-joint welded parts made of an austenitic stainless steel 304 L and a duplex stainless steel S31803. Walbridge introduced a strain-based fracture mechanics model [122] for investigating the effect of needle peening on bridge structures under variable loading conditions [83]. The model is based on Paris–Erdogan crack growth law which is commonly used in linear elastic fracture mechanics. Fig. 18 shows that the method delays crack growth [123] and hence prolonged fatigue life and strength. Being able to predict two main accelerating crack growth mechanisms, i.e. reducing the crack opening stress level by large compressive loads and relaxing compressive residual stresses induced by the peening process because of the non-linear material behaviors, this model was later used to model UPT. The effect of UPT under-treatment, proper, and over-treatment was investigated by Walbridge et al. [93] both experimentally (see Fig. 11) and numerically with the help of 2D FEM simulation using the ABAQUS software program. By reducing the UPT intensity (from 27–29 μm down to 18 μm) or increasing the treatment speed (from 10 to 20 mm/s), under-treatment was simulated. Over-treatment, however, was modeled by reducing the treatment speed to 1 mm/s. The proper treatment was assumed to have a treatment speed of 10 mm/s and treatment amplitude of 27–29 μm. Through their research, a strong relation was found between the UPT performance and both the level of residual stresses and microhardness. For verifying under treated weld toes, indent depth values and any traces of the original weld toe should be taken into account. However, for the over-treated weld toes, the weld toe severe damage or flaking evidences are effective practical means. In 2012, based on Gurson–Tvergaard–Needleman ductile damage constitutive equations, the damage induced by the UPT was studied by Yang et al. [124] and then they concluded that the collision of material surface and the impact tool may cause the microstructure damage when peening of AISI-304 stainless steel samples. The impact velocities employed were 3 m/s, 4 m/s and 5 m/s, respectively. The Gurson–Tvergaard–Needleman model is described below [125]. σ 2e 3σ m 2 − 1 þ q3 ð f Þ ¼ 0 þ 2q f cosh q 1 2 2σ y σ 2y ð1Þ σe, σy and σm are Von-Mises, yield, and mean stresses, respectively. f * is the void volume fraction parameter describing void coalescence. M. Malaki, H. Ding / Materials and Design 87 (2015) 1072–1086 1083 Fig. 20. Impact models: (a) single-impact model and (b): two-impact model [127]. q1, q2, and q3 are all the constitutive factors. The peening impact was calculated by the following formula [126]. P≈ i fi h 2 2 2 2π f us ξ mp þ Er m ð2Þ where P is the mechanical energy per impact and fi ≈ 3 ± 0.5 kHz is the impacting frequency. As a correlation between pin mass (mp) and sample mass (ms), m is a coefficient with mass dimension. fus and ξ are vibration amplitude and frequency of the vibrating horn respectively. Er is the pin energy acquired from the movement of the mechanical head or specimen itself. According to the results, maximum compressive residual stresses are created at the depth of 0.2 mm in different impact velocities, i.e. 3 m/s, 4 m/s and 5 m/s. However, it was found that both the magnitude and the thickness of the layer of exerted compressive residual stresses are severely affected by the impact velocity. Also, they showed that the damage depth is only about 0.07 mm. If a layer with thickness of about 0.1 mm could be removed from the treated surface, not only will the material surface be free of any damages but also a layer of hardened material will be kept on the surface [124]. Using the modified strip-yielding model, Shimanuki and Okawa [113] simulated residual stresses caused by welding or the UPT treatment and found that improving fatigue strength post treatment by the UPT is a superior technique than that of grinding especially for stress ratios lower than 0.5. Fig. 19 shows also a comparison between the estimated S–N curves with the experimental fatigue test values. Recently, a new FEM simulation of UPT is done by Chaobo et al. studying two 3D FEM models in the ABAQUS/Explicit environment [127]. Using Johnson–Cook equation, the effects of impact velocity, pin size, and shape on the amount of residual stresses and strains exerted on the surface of 2024 aluminum alloy were studies in this work. Fig. 20 shows the two impact models, i.e. single-impact model and two-impact model. Fig. 21 shows the residual stress field in the two models. As it is clear, there haven't been many numerically computer-based simulation studies reported so far. It may be caused by the following factors. Exact deformation behavior of the UPT treated materials is complicated, and there are many material non-linearites and unknown phenomena which cannot be simulated by the current FEM tools. Further investigations are critically needed for the understanding of grains deformation, material softening, strain-induced residual stresses, phase Fig. 21. Residual stress field. (a): Single-impact, (b): D = 0.05 mm, (c): D = 0.4 mm, (d): D = 1.2 mm (D is pin distances) [127]. 1084 M. Malaki, H. Ding / Materials and Design 87 (2015) 1072–1086 recrystallizations and fracture mechanics of ultrasonically peened materials. The more in-depth the process can be understood, the better the process could be simulated. 7. Conclusions In the current review paper, Ultrasonic Peening Treatment (UPT) was discussed and its effects on the micro-structure, hardness, corrosion and fatigue strength and life have been explained with the help of almost all research works reported so far. It was concluded that both metallurgical and mechanical aspects can be enhanced while using the UPT. The method can effectively prolong fatigue life and enhance fatigue strength of steel structures significantly. The UPT makes the structures more resilient against corrosive liquids and solutions like sea water; a layer of very hard strain-induced Nanocrystalline material is generated on the surface through ultrasonic impacts; micro-cracks, voids, cavities and or any kind of impurities can be closed and peened with the help of ultrasonic peening assistance. Finally, it was shown that the UPT is able to substantially improve mechanical strength of the steel structures, especially high strength steels. For those of light weight structures such as aluminum alloys, further investigations are needed. References [1] M.P. Nascimento, R.C. Souza, W.L. Pigatin, H.J.C. Voorwald, Effects of surface treatments on the fatigue strength of AISI 4340 aeronautical steel, Int. J. Fatigue 23 (7) (2001) 607–618. [2] K. Kirkhope, R. Bell, L. Caron, R. Basu, K.-T. Ma, Weld detail fatigue life improvement techniques. Part 2: application to ship structures, Mar. Struct. 12 (7) (1999) 477–496. [3] T. Deguchi, M. Mouri, J. Hara, D. Kano, T. Shimoda, F. Inamura, T. Fukuoka, K. Koshio, Fatigue strength improvement for ship structures by Ultrasonic Peening, J. Mar. Sci. Technol. 17 (3) (2012) 360–369. [4] L.L. Martinez, Z. Barsoum, A. Paradowska, State-of-the-art: fatigue life extension of offshore installations, ASME 2012 31st International Conference on Ocean, Offshore and Arctic Engineering, American, Society of Mechanical Engineers 2012, pp. 9–20. [5] Y. Kudryavtsev, J. Kleiman, Application of Ultrasonic Peening for Fatigue Life Improvement of Automotive Welded Wheels, International Institute of Welding, 2005 (IIW Document XIII-2075-05, 9 pp.). [6] S. Maddox, M.J. Doré, S. Smith, A Case Study Of The Use Of Ultrasonic Peening For Upgrading A Welded Steel Structure, Weld. World 55 (9–10) (2011) 56–67. [7] D. Yin, D. Wang, H. Jing, L. Huo, The effects of ultrasonic peening treatment on the ultralong life fatigue behavior of welded joints, Mater. Des. 31 (7) (2010) 3299–3307. [8] M. Shalvandi, Y. Hojjat, A. Abdullah, H. Asadi, Influence of ultrasonic stress relief on stainless steel 316 specimens: A comparison with thermal stress relief, Mater. Des. 46 (2013) 713–723. [9] I. Mukhanov, Y.M. Golubev, Strengthening Steel Components by Ultrasonically Vibrating Ball, Vestn. Mashin. 11 (1966) 52–53. [10] N. Krylov, A. Polischuk, The use of ultrasonic equipment for metal structure stabilization, Basic Physics of Industrial Ultrasonic Applications, Part, 11970 70. [11] K. Kirkhope, R. Bell, L. Caron, R. Basu, K.-T. Ma, Weld detail fatigue life improvement techniques. Part 1: review, Mar. Struct. 12 (6) (1999) 447–474. [12] J. Knight, Improving the fatigue strength of fillet welded joints by grinding and peening, Weld. Res. Int. 8 (6) (1978) 519–540. [13] T. Gurney, Effect of peening and grinding on the fatigue strength of fillet welded joints, Br. Weld. J. 15 (12) (1968) 601–609. [14] E.S. Statnikov, O.V. Korolkov, V.O. Muktepavel, V.Y. Korostel, Oscillating system and tool for ultrasonic impact treatment, US Patent, Patent No. 20080035627-A1, UIT L.L.C., United States, 2007. [15] E. Statnikov, V. Korostel, V. Vityazev, O. Korolkov, Method of improving quality and reliability of welded rail joint properties by ultrasonic impact treatment, US Patent, Patent No.US 20060016858-A1, UIT L.L.C., United States, 2006. [16] P. Mikheev, E. Garf, A. Kuz'menko, V. Zaitsev, E.S. Statnikov, Improvement of fatigue resistance of tubular welded connections by ultrasonic peening, Int. J. Offshore Polar Eng. 6 (4) (1996) 1–4. [17] C.M. Branco, V. Infante, R. Baptista, Fatigue behaviour of welded joints with cracks, repaired by hammer peening, Fatigue Fract. Eng. Mater. Struct. 27 (9) (2004) 785–798. [18] L. Hacini, N. Van Lê, P. Bocher, Effect of impact energy on residual stresses induced by hammer peening of 304 L plates, J. Mater. Process. Technol. 208 (1–3) (2008) 542–548. [19] I.E. Kopsov, The influence of hammer peening on fatigue in high-strength steel, Int. J. Fatigue 13 (6) (1991) 479–482. [20] R. Baptista, V. Infante, C. Branco, Fully Dynamic Numerical Simulation of the Hammer Peening Fatigue Life Improvement Technique, Procedia Eng. 10 (2011) 1943–1948. [21] L. Hacini, N. Lê, P. Bocher, Evaluation of Residual Stresses Induced by Robotized Hammer Peening by the Contour Method, Exp. Mech. 49 (6) (2009) 775–783. [22] V.-M. Lihavainen, G. Marquis, E. Statnikov, Fatigue strength of a longitudinal attachment improved by ultrasonic impact treatment, Weld. World 48 (5–6) (2004) 67–73. [23] G.H. Farrahi, H. Ghadbeigi, An investigation into the effect of various surface treatments on fatigue life of a tool steel, J. Mater. Process. Technol. 174 (1–3) (2006) 318–324. [24] P. Sarvi Hampa, M. Razfar, M. Malaki, A. Maleki, The Role of Dry Aero-acoustical Lubrication and Material Softening in Ultrasonically Assisted Milling of Difficultto-Cut AISI 304 Steels, Trans. Indian Inst. Metals 68 (1) (2015) 43–49. [25] K. Dalaei, B. Karlsson, Influence of shot peening on fatigue durability of normalized steel subjected to variable amplitude loading, Int. J. Fatigue 38 (2012) 75–83. [26] H. Ding, Y.C. Shin, Dislocation density-based modeling of subsurface grain refinement with laser-induced shock compression, Comput. Mater. Sci. 53 (1) (2012) 79–88. [27] Y. Gao, B. Wu, Z. Liu, Y. Zhou, N. Shen, H. Ding, Ultrasonic Cavitation Peening of Stainless Steel and Nickel Alloy, J. Manuf. Sci. Eng. 136 (1) (2014) 014502. [28] A. Abdullah, M. Malaki, E. Baghizadeh, On the impact of ultrasonic cavitation bubbles, Proc. Inst. Mech. Eng. C J. Mech. Eng. Sci. 226 (3) (2012) 681–694. [29] Y. Liu, D. Wang, C. Deng, L. Xia, L. Huo, L. Wang, B. Gong, Influence of re-ultrasonic impact treatment on fatigue behaviors of S690QL welded joints, Int. J. Fatigue 66 (2014) 155–160. [30] A. Abdullah, M. Malaki, A. Eskandari, Strength enhancement of the welded structures by ultrasonic peening, Mater. Des. 38 (2012) 7–18. [31] E.S. Statnikov, V. Muktepavel, Technology of ultrasound impact treatment as a means of improving the reliability and endurance of welded metal structures, Weld. Int. 17 (9) (2003) 741–744. [32] S. Roy, J.W. Fisher, B.T. Yen, Fatigue resistance of welded details enhanced by ultrasonic impact treatment (UIT), Int. J. Fatigue 25 (9) (2003) 1239–1247. [33] Y. Kudryavtsev, J. Kleiman, A. Lugovskoy, G. Prokopenko, Fatigue Life Improvement of Tubular Welded Joints by Ultrasonic Peening, International Institute of Welding, 2006 (IIW Document XIII-2117-06, 24 pp.). [34] G. Prokopenko, A.Y. Nedoseka, A. Gruzd, T. Krasovskii, Development and optimization of the equipment and process of ultrasonic impact treatment of welded joints for the reduction of residual stresses, Tekh. Diagn. Nerazrush. Kontrol (3) (1995) 14–22. [35] B.N. Mordyuk, G.I. Prokopenko, M.A. Vasylyev, M.O. Iefimov, Effect of structure evolution induced by ultrasonic peening on the corrosion behavior of AISI-321 stainless steel, Mater. Sci. Eng. A 458 (1–2) (2007) 253–261. [36] L.M. Lobanov, V.I. Kyr'yan, V.V. Knysh, Enhancement of the service life of welded metal structures by high-frequency mechanical peening, Mater. Sci. 42 (1) (2006) 54–60. [37] G.I. Prokopenko, O.I. Kozlov, J.I. Kleiman, P.P. Micheev, V.V. Knysh, Y.F. Kudryavtsev, Device for ultrasonic peening of metals, US Patent, No. US6467321-B2, Integrity Testing Laboratory, Inc., United States, 2002. [38] B.N. Mordyuk, G.I. Prokopenko, Ultrasonic impact peening for the surface properties' management, J. Sound Vib. 308 (3–5) (2007) 855–866. [39] M. Malaki, A. Abdullah, Analytically Non-Classic Design of a Piezoelectric Resonator, U.P.B. Sci. Bull. Ser. A Appl. Math. Phys. 74 (4) (2012) 183–194. [40] A. Abdullah, A. Pak, Correct Prediction of the Vibration Behavior of a High Power Ultrasonic Transducer by FEM Simulation, Int. J. Adv. Manuf. Technol. 39 (1–2) (2008) 21–28. [41] A. Abdullah, A. Pak, M. Abdullah, A. Shahidi, M. Malaki, Study of the behavior of ultrasonic piezo-ceramic actuators by simulations, Electron. Mater. Lett. 10 (1) (2014) 37–42. [42] V.K. Astashev, K. Khusnutdinova, V. Babitsky, Ultrasonic Processes and Machines: Dynamics, Control and Applications, Springer, 2007. [43] K. Nakamura, Ultrasonic Transducers: Materials and Design for Sensors, Actuators and Medical Applications, Elsevier, 2012. [44] A. Abdullah, M. Malaki, On the damping of ultrasonic transducers' components, Aerosp. Sci. Technol. 28 (1) (2013) 31–39. [45] Y. Kudryavtsev, J. Kleiman, A. Lugovskoy, L. Lobanov, V. Knysh, O. Voitenko, G. Prokopenko, Rehabilitation and Repair of Welded Elements and Structures by Ultrasonic Peening, Weld. World 51 (7–8) (2007) 47–53. [46] Y. Kudryavtsev, J. Kleiman, L. Lobanov, V. Knysh, G. Prokopenko, Fatigue life improvement of welded elements by ultrasonic peening, International Institute of Welding, 2004 (IIW Document XIII-2010-04, 20 pp.). [47] B. Langenecker, Effects of Ultrasound on Deformation Characteristics of Metals, IEEE Trans. Son. Ultrason. 13 (1) (1966) 1–8. [48] A. Siddiq, E. Ghassemieh, Thermomechanical analyses of ultrasonic welding process using thermal and acoustic softening effects, Mech. Mater. 40 (12) (2008) 982–1000. [49] A. Siddiq, T. El Sayed, Acoustic softening in metals during ultrasonic assisted deformation via CP-FEM, Mater. Lett. 65 (2) (2011) 356–359. [50] A. Siddiq, T. El Sayed, Ultrasonic-assisted manufacturing processes: Variational model and numerical simulations, Ultrasonics 52 (4) (2012) 521–529. [51] S. Statnikov, Guide for application of ultrasonic impact treatment improving fatigue life of welded structures, Proc. Life of Welded Structures, IIW/IIS-DOCUMENT XIII-1757–99, 1999 Russia. [52] L. Wagner, Mechanical surface treatments on titanium, aluminum and magnesium alloys, Mater. Sci. Eng. A 263 (2) (1999) 210–216. [53] S. Roy, J.W. Fisher, Enhancing fatigue strength by ultrasonic impact treatment, Int. J. Steel Struct. 5 (3) (2005) 241–252. [54] T.-L. Teng, C.-P. Fung, P.-H. Chang, Effect of weld geometry and residual stresses on fatigue in butt-welded joints, Int. J. Press. Vessel. Pip. 79 (7) (2002) 467–482. M. Malaki, H. Ding / Materials and Design 87 (2015) 1072–1086 [55] X.J. Hu, X.H. Li, Q.Y. Qin, Influence of Ultrasonic Vibration on Metal Plastic Forming, Appl. Mech. Mater. 470 (2014) 162–169. [56] M. Turski, S. Clitheroe, A.D. Evans, C. Rodopoulos, D.J. Hughes, P.J. Withers, Engineering the residual stress state and microstructure of stainless steel with mechanical surface treatments, Appl. Phys. A 99 (3) (2010) 549–556. [57] X. Cheng, J.W. Fisher, H.J. Prask, T. Gnäupel-Herold, B.T. Yen, S. Roy, Residual stress modification by post-weld treatment and its beneficial effect on fatigue strength of welded structures, Int. J. Fatigue 25 (9) (2003) 1259–1269. [58] J. Janosch, H. Koneczny, S. Debiez, E. Statnikov, V. Troufiakov, P. Mikhee, Improvement of fatigue strength in welded joints (in HSS and in aluminium alloys) by ultrasonic hammer peening, Int. J. Fatigue 19 (10) (1997) 725. [59] X. An, C.A. Rodopoulos, E.S. Statnikov, V.N. Vitazev, O.V. Korolkov, Study of the surface nanocrystallization induced by the esonix ultrasonic impact treatment on the near-surface of 2024-T351 aluminum alloy, J. Mater. Eng. Perform. 15 (3) (2006) 355–364. [60] Q.F. Zhu, Z.M. Sun, T.D. Ma, V.A. Klimenov, V. Borozna, B.H. Zhu, Effect of ultrasonic surface peening on fatigue property of 7B04 high strength and toughness aluminum alloy, Proc. Materials Science Forum, Trans Tech Publ (2010) 1892–1895. [61] B.N. Mordyuk, G.I. Prokopenko, Fatigue life improvement of α-titanium by novel ultrasonically assisted technique, Mater. Sci. Eng. A 437 (2) (2006) 396–405. [62] T. Roland, D. Retraint, K. Lu, J. Lu, Fatigue life improvement through surface nanostructuring of stainless steel by means of surface mechanical attrition treatment, Scr. Mater. 54 (11) (2006) 1949–1954. [63] Z. Fan, H. Xu, D. Li, L. Zhang, L. Liao, Surface Nanocrystallization of 35# Type Carbon Steel Induced by Ultrasonic Impact Treatment (UIT), Procedia Eng. 27 (2012) 1718–1722. [64] I. Weich, T. Ummenhofer, T. Nitschke-Pagel, K. Dilger, H. Eslami Chalandar, Fatigue Behaviour of Welded High-Strength Steels after High Frequency Mechanical Post-Weld Treatments, Weld. World 53 (11–12) (2009) R322–R332. [65] K.A. Darling, M.A. Tschopp, A.J. Roberts, J.P. Ligda, L.J. Kecskes, Enhancing grain refinement in polycrystalline materials using surface mechanical attrition treatment at cryogenic temperatures, Scr. Mater. 69 (6) (2013) 461–464. [66] C.-M. Suh, G.-H. Song, M.-S. Suh, Y.-S. Pyoun, Fatigue and mechanical characteristics of nano-structured tool steel by ultrasonic cold forging technology, Mater. Sci. Eng. A 443 (1–2) (2007) 101–106. [67] A. Cherif, Y. Pyoun, B. Scholtes, Effects of Ultrasonic Nanocrystal Surface Modification (UNSM) on Residual Stress State and Fatigue Strength of AISI 304, J. Mater. Eng. Perform. 19 (2) (2010) 282–286. [68] X.H. Chen, J. Lu, L. Lu, K. Lu, Tensile properties of a nanocrystalline 316 L austenitic stainless steel, Scr. Mater. 52 (10) (2005) 1039–1044. [69] S.-H. Han, J.-W. Han, Y.-Y. Nam, I.-H. Cho, Fatigue life improvement for cruciform welded joint by mechanical surface treatment using hammer peening and UNSM, in: S. Pantelakis, C. Rodopoulos (Eds.), Engineering Against Fracture, Springer, Netherlands 2009, pp. 411–419. [70] M. Daavari, S.A. Sadough Vanini, Corrosion fatigue enhancement of welded steel pipes by ultrasonic impact treatment, Mater. Lett. 139 (2015) 462–466. [71] T. Wang, J. Yu, B. Dong, Surface nanocrystallization induced by shot peening and its effect on corrosion resistance of 1Cr18Ni9Ti stainless steel, Surf. Coat. Technol. 200 (16–17) (2006) 4777–4781. [72] X.Y. Wang, D.Y. Li, Mechanical and electrochemical behavior of nanocrystalline surface of 304 stainless steel, Electrochim. Acta 47 (24) (2002) 3939–3947. [73] H.-s. Lee, D.-s. Kim, J.-s. Jung, Y.-s. Pyoun, K. Shin, Influence of peening on the corrosion properties of AISI 304 stainless steel, Corros. Sci. 51 (12) (2009) 2826–2830. [74] F. Bleicher, C. Lechner, C. Habersohn, E. Kozeschnik, B. Adjassoho, H. Kaminski, Mechanism of surface modification using machine hammer peening technology, CIRP Ann. Manuf. Technol. 61 (1) (2012) 375–378. [75] J.O. Peters, B.L. Boyce, A.W. Thompson, R.O. Ritchie, O. Roder, Role of foreign-object damage on thresholds for high-cycle fatigue in Ti–6Al–4V, Metall. Mater. Trans. A 31 (6) (2000) 1571–1583. [76] J.-H. Kim, M.-G. Kim, Considerations in non-propagating crack of pure titanium, Mater. Sci. Eng. A 346 (1–2) (2003) 216–222. [77] A. Barbucci, M. Delucchi, M. Panizza, M. Sacco, G. Cerisola, Electrochemical and corrosion behaviour of cold rolled AISI 301 in 1 M H2SO4, J. Alloys Compd. 317–318 (2001) 607–611. [78] P. Haagensen, E. Statnikov, L. Lopez-Martinez, Introductory fatigue tests on welded joints in high strength steel and aluminium improved by various methods including ultrasonic impact treatment (UIT), IIW Doc, 13 1998, pp. 1748–1798. [79] P. Haagensen, S. Maddox, IIW recommendations on post weld improvement of steel and aluminium structures, IIW document, 13, International Institute of Welding 2001, pp. 1815–1820. [80] V. Trufiakov, E. Statnikov, P. Mikheev, A. Kuzmenko, The Efficiency of Ultrasonic Impact Treatment for Improving the Fatigue Strength of Welded Joints, IIW Document, 13, International Institute of Welding 1998, pp. 1745–1798. [81] M. Castillo-Morales, A. Salas-Zamarripa, The effects of UIT in the fatigue life of Al 2024-T3, Key Eng. Mater. 449 (2010) 15–22. [82] C. Miki, M. Tai, Fatigue strength improvement of out-of-plane welded joints of steel girder under variable amplitude loading, Weld. World 57 (6) (2013) 823–840. [83] K. Ghahremani, S. Walbridge, Fatigue testing and analysis of peened highway bridge welds under in-service variable amplitude loading conditions, Int. J. Fatigue 33 (3) (2011) 300–312. [84] M. Tai, C. Miki, Improvement Effects of Fatigue Strength by Burr Grinding and Hammer Peening Under Variable Amplitude Loading, Weld. World 56 (7–8) (2012) 109–117. 1085 [85] H.C. Yildirim, G.B. Marquis, Fatigue strength improvement factors for high strength steel welded joints treated by high frequency mechanical impact, Int. J. Fatigue 44 (2012) 168–176. [86] E.S. Statnikov, V.O. Muktepavel, A. Blomqvist, Comparison of Ultrasonic Impact Treatment (UIT) and Other Fatigue Life Improvement Methods, Weld. World 46 (3–4) (2002) 20–32. [87] S.W. Ooi, J.E. Garnham, T.I. Ramjaun, Review: Low transformation temperature weld filler for tensile residual stress reduction, Mater. Des. 56 (2014) 773–781. [88] H. Lixing, W. Dongpo, W. Wenxian, Z. Yufeng, Ultrasonic Peening and Low Transformation Temperature Electrodes used for Improving the Fatigue Strength of Welded Joints, Weld. World 48 (3–4) (2004) 34–39. [89] T. Tominaga, K. Matsuoka, Y. Sato, T. Suzuki, Fatigue Improvement of Weld Repaired Crane Runway Girder by Ultrasonic Impact Treatment, Weld. World 52 (11–12) (2008) 50–62. [90] C. Shiga, E. Murakawa, Y. Matsuo, U. Ohsuga, K. Hiraoka, Y. Morikage, K. Yasuda, Fatigue improvement in high-strength steel welded joints with compressive residual stress, Weld. World 58 (1) (2014) 55–64. [91] A. Galtier, E.S. Statnikov, The Influence of Ultrasonic Impact Treatment on Fatigue Behaviour of Welded Joints in High-Strength Steel, Weld. World 48 (5–6) (2004) 61–66. [92] E.S. Statnikov, O.V. Korolkov, V.N. Vityazev, Physics and mechanism of ultrasonic impact, Ultrasonics 44 (2006) e533–e538. [93] R. Tehrani Yekta, K. Ghahremani, S. Walbridge, Effect of quality control parameter variations on the fatigue performance of ultrasonic impact treated welds, Int. J. Fatigue 55 (2013) 245–256. [94] L. Huo, D. Wang, Y. Zhang, Investigation of the fatigue behaviour of the welded joints treated by TIG dressing and ultrasonic peening under variable-amplitude load, Int. J. Fatigue 27 (1) (2005) 95–101. [95] B.N. Mordyuk, Y.V. Milman, M.O. Iefimov, G.I. Prokopenko, V.V. Silberschmidt, M.I. Danylenko, A.V. Kotko, Characterization of ultrasonically peened and laser-shock peened surface layers of AISI 321 stainless steel, Surf. Coat. Technol. 202 (19) (2008) 4875–4883. [96] B.N. Mordyuk, O.P. Karasevskaya, G.I. Prokopenko, Structurally induced enhancement in corrosion resistance of Zr–2.5%Nb alloy in saline solution by applying ultrasonic impact peening, Mater. Sci. Eng. A 559 (2013) 453–461. [97] X. Zhao, D. Wang, L. Huo, Analysis of the S–N curves of welded joints enhanced by ultrasonic peening treatment, Mater. Des. 32 (1) (2011) 88–96. [98] G.R. Jinu, P. Sathiya, G. Ravichandran, A. Rathinam, Investigation of the fatigue behaviour of butt-welded joints treated by ultrasonic peening process and compared with fatigue life assessment standards, Int. J. Adv. Manuf. Technol. 40 (1–2) (2009) 74–83. [99] M. Pedersen, O. Mouritsen, M. Hansen, J. Andersen, J. Wenderby, Comparison of Post-Weld Treatment of High-Strength Steel Welded Joints in Medium Cycle Fatigue, Weld. World 54 (7–8) (2010) R208–R217. [100] W.Z. Zhuang, G.R. Halford, Investigation of residual stress relaxation under cyclic load, Int. J. Fatigue 23 (Supplement 1) (2001) 31–37. [101] B. BS 7608: 1993 Code of Practice for Fatigue Design and Assessment of Steel Structures, British Standards Institution, London, 1995. [102] AWS, Structural Welding Code Steel, American Welding Society (AWS), 2006. [103] A. Hobbacher, Recommendations for Fatigue Design of Welded Joints and Components, International Institute of Welding, 2002 (IIW doc. XIII-153996/XV-845-96). [104] T. Wang, D. Wang, L. Huo, Y. Zhang, Discussion on fatigue design of welded joints enhanced by ultrasonic peening treatment (UPT), Int. J. Fatigue 31 (4) (2009) 644–650. [105] M.D. Chapetti, T. Tagawa, T. Miyata, Ultra-long cycle fatigue of high-strength carbon steels part I: review and analysis of the mechanism of failure, Mater. Sci. Eng. A 356 (1–2) (2003) 227–235. [106] M.D. Chapetti, T. Tagawa, T. Miyata, Ultra-long cycle fatigue of high-strength carbon steels part II: estimation of fatigue limit for failure from internal inclusions, Mater. Sci. Eng. A 356 (1–2) (2003) 236–244. [107] R.L. Carlson, G.A. Kardomateas, J.I. Craig, Mechanics of Failure Mechanisms in Structures, Springer, 2012. [108] A.A. Shanyavskiy, Mechanisms and modeling of subsurface fatigue cracking in metals, Eng. Fract. Mech. 110 (2013) 350–363. [109] Y.-H. Zhang, S.J. Maddox, Fatigue life prediction for toe ground welded joints, Int. J. Fatigue 31 (7) (2009) 1124–1136. [110] P. Zerres, M. Vormwald, Review of fatigue crack growth under non-proportional mixed-mode loading, Int. J. Fatigue 58 (2014) 75–83. [111] A.F. Hobbacher, The new IIW recommendations for fatigue assessment of welded joints and components — A comprehensive code recently updated, Int. J. Fatigue 31 (1) (2009) 50–58. [112] T. Mori, H. Shimanuki, M. Tanaka, Effect Of Uit On Fatigue Strength Of Web-Gusset Welded Joints Considering Service Condition Of Steel Structures, Weld. World 56 (9–10) (2012) 141–149. [113] H. Shimanuki, T. Okawa, Effect of stress ratio on the enhancement of fatigue strength in high performance steel welded joints by ultrasonic impact treatment, Int. J. Steel Struct. 13 (1) (2013) 155–161. [114] Q.L. Yang, D.P. Wang, S.P. Wu, S. Li, Research on the Effect of Ultrasonic Impact Peening on the Fatigue Property of 7075-T651 Aluminum Alloy, Adv. Mater. Res. 295 (2011) 1896–1900. [115] T. Okawa, H. Shimanuki, Y. Funatsu, T. Nose, Y. Sumi, Effect of preload and stress ratio on fatigue strength of welded joints improved by ultrasonic impact treatment, Weld. World 57 (2) (2013) 235–241. [116] B.N. Mordyuk, M.O. Iefimov, G.I. Prokopenko, T.V. Golub, M.I. Danylenko, Structure, microhardness and damping characteristics of Al matrix composite reinforced with 1086 M. Malaki, H. Ding / Materials and Design 87 (2015) 1072–1086 AlCuFe or Ti using ultrasonic impact peening, Surf. Coat. Technol. 204 (9–10) (2010) 1590–1598. [117] G. Marquis, E. Mikkola, H. Yildirim, Z. Barsoum, Fatigue strength improvement of steel structures by high-frequency mechanical impact: proposed fatigue assessment guidelines, Weld. World 57 (6) (2013) 803–822. [118] M. Liao, W.R. Chen, N.C. Bellinger, Effects of ultrasonic impact treatment on fatigue behavior of naturally exfoliated aluminum alloys, Int. J. Fatigue 30 (4) (2008) 717–726. [119] B. Atzori, G. Meneghetti, Fatigue strength of fillet welded structural steels: finite elements, strain gauges and reality, Int. J. Fatigue 23 (8) (2001) 713–721. [120] J. Liu, W.X. Gou, W. Liu, Z.F. Yue, Effect of hammer peening on fatigue life of aluminum alloy 2A12-T4, Mater. Des. 30 (6) (2009) 1944–1949. [121] G. Quilliec, H.-P. Lieurade, M. Bousseau, M. Drissi-Habti, G. Inglebert, P. Macquet, L. Jubin, Mechanics and modelling of high-frequency mechanical impact and its effect on fatigue, Weld. World 57 (1) (2013) 97–111. [122] S. Walbridge, Fatigue analysis of post-weld fatigue improvement treatments using a strain-based fracture mechanics model, Eng. Fract. Mech. 75 (18) (2008) 5057–5071. [123] M. Tai, C. Miki, K. Suzuki, Mechanism of Fatigue Strength Improvement by Applying Peening Treatment, Procedia Eng. 14 (2011) 117–125. [124] X. Yang, J. Zhou, X. Ling, Study on plastic damage of AISI 304 stainless steel induced by ultrasonic impact treatment, Mater. Des. 36 (2012) 477–481. [125] V. Tvergaard, A. Needleman, Analysis of the cup-cone fracture in a round tensile bar, Acta Metall. 32 (1) (1984) 157–169. [126] A.C. Sekkal, C. Langlade, A.B. Vannes, Tribologically transformed structure of titanium alloy (TiAl6V4) in surface fatigue induced by repeated impacts, Mater. Sci. Eng. A 393 (1–2) (2005) 140–146. [127] C. Guo, Z. Wang, D. Wang, S. Hu, Numerical analysis of the residual stress in ultrasonic impact treatment process with single-impact and two-impact models, Appl. Surf. Sci. 347 (2015) 596–601. Update Materials & Design Volume 91, Issue , 5 February 2016, Page 442 DOI: https://doi.org/10.1016/j.matdes.2015.11.108 Materials and Design 91 (2016) 442 Contents lists available at ScienceDirect Materials and Design journal homepage: www.elsevier.com/locate/matdes Corrigendum Corrigendum to “A review of ultrasonic peening treatment” [Mater. Des. 87 (2015) 1072–1086] Massoud Malaki a,⁎, Hongtao Ding b a b Young Researchers and Elite Club, Najafabad Branch, Islamic Azad University, Najafabad, Isfahan, Iran Mechanical and Industrial Engineering Department, University of Iowa, Iowa City, IA 52242, USA The authors regret to inform that Massoud Malaki's correct affiliation is “Young Researchers and Elite Club, Najafabad Branch, Islamic Azad University, Najafabad, Isfahan, Iran”. The authors would like to apologize for the inconvenience caused. DOI of original article: http://dx.doi.org/10.1016/j.matdes.2015.08.102. ⁎ Corresponding author. Tel./fax: +98 912 4424739. E-mail addresses: massoudmalaki@gmail.com, m.malaki@iut.ac.ir (M. Malaki). http://dx.doi.org/10.1016/j.matdes.2015.11.108 0264-1275/© 2015 Elsevier Ltd. All rights reserved.
0
You can add this document to your study collection(s)
Sign in Available only to authorized usersYou can add this document to your saved list
Sign in Available only to authorized users(For complaints, use another form )